Electrode assembly and manufacturing method therefor

The zigzag electrode assembly addresses adhesion-related bending issues by optimizing the adhesion between the separator and electrodes, ensuring improved safety and performance through uniform adhesion forces and maintaining high productivity and energy density.

WO2024228503A1PCT designated stage expired Publication Date: 2024-11-07LG ENERGY SOLUTION LTD

Patent Information

Application Number
PCT/KR2024/005396
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-02
Filing Date
2024-04-22
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Conventional zigzag electrode assemblies experience bending issues due to differences in adhesion between the separator and electrodes, leading to potential separation and reduced stiffness, which can cause safety concerns and affect the performance of electrochemical devices.

Method used

The electrode assembly features a zigzag separator with a porous substrate and distinct porous coating layers on each side, optimizing the adhesion between the cathode and anode surfaces to maintain uniform adhesion forces, thereby reducing bending and enhancing the structural integrity of the device.

Benefits of technology

This configuration ensures improved safety and performance of electrochemical devices by minimizing adhesion differences and maintaining the advantages of zigzag stacking, such as high productivity and energy density, while preventing electrode and separator detachment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005396_07112024_PF_FP_ABST
    Figure KR2024005396_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides an electrode assembly comprising: a separator curved in a zigzag shape; an anode arranged between first surfaces of the separator; and a cathode arranged between second surfaces of the separator, wherein: each of the cathode and the anode has a top surface and a bottom surface having a surface adhesion lower than that of the top surface; and the top surface of the cathode is arranged to face the top surface of the anode with the separator therebetween so that bending is structurally reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode assembly and method for manufacturing the same

[0001] This application claims priority based on Korean Patent Application No. 10-2023-0057042, filed with the Korean Intellectual Property Office on May 2, 2023, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to an electrode assembly including a zigzag-shaped separator and a method for manufacturing the same.

[0003] Electrochemical devices convert chemical energy into electrical energy using electrochemical reactions. Recently, lithium secondary batteries have become widely used due to their high energy density and voltage, long cycle life, and wide range of applications. With the increasing demand for electric vehicles and energy storage devices, development is underway on materials and structures to maximize capacity and energy density.

[0004] A secondary battery may include an electrode assembly including a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode, and may be manufactured by housing the electrode assembly in a case together with an electrolyte. Secondary batteries may be classified into pouch-type, cylindrical, square, coin-type, etc. depending on the shape of the case in which the electrode assembly is housed, and may be classified into jelly-roll type, stack type, etc. depending on the manufacturing method or shape of the electrode assembly.

[0005] Recently, a zigzag stacking electrode assembly has been developed, which folds a long sheet-shaped separator in a zigzag shape and alternately places positive and negative electrodes between adjacent folds. For example, a zigzag electrode assembly can be manufactured by tilting or swinging a table on which an elongated sheet-shaped separator is stacked when supplied, or by reciprocating a feed roll that transports the separator to fold the separator in a zigzag shape and place each electrode between the folds. Zigzag stacking has the advantage of being simpler than other types of processes, resulting in superior productivity.

[0006] The separator used in zigzag stacking can be formed by coating a coating slurry on both sides of a porous substrate, and the electrode can be formed by coating an active material slurry on both sides of an electrode current collector. Even if the separator is coated and dried on both sides simultaneously, there may be differences in the drying time between the upper and lower surfaces, resulting in differences in adhesive strength on each surface. The electrode is sequentially coated and dried with each active material layer, and the first coated layer passes through the drying oven twice, which may result in differences in adhesive strength on each surface. For this reason, adhesive strength may vary depending on the surface of the separator and electrode, despite the adjustment of the coating conditions.

[0007] Referring to FIG. 1, a conventional zigzag-shaped electrode assembly (1) has a structure in which a negative electrode (10) and a positive electrode (20) are alternately arranged between zigzag-folded separators (30). The negative electrode (10) includes an upper surface (11) and a lower surface (12) coated on each surface of a negative electrode current collector (13), and the positive electrode (20) includes an upper surface (21) and a lower surface (22) coated on each surface of a positive electrode current collector (23). The thickness of the upper surface of each electrode may be greater than the thickness of the lower surface, or the surface adhesive force of the upper surface may be greater than the surface adhesive force of the lower surface. In this case, the lower surface (12) of the negative electrode may face the upper surface (21) of the positive electrode with the separator (30) interposed therebetween, and the upper surface (11) of the negative electrode may face the lower surface (22) of the positive electrode with the separator (30) interposed therebetween. In the above arrangement, since the adhesive strength applied to both sides of the separator (30) is different, bending of the zigzag electrode assembly during the manufacturing process or the manufactured one may occur. For example, the adhesive strengths of the contact surface b and the contact surface c may be different, and the electrode assembly may bend toward the c side where the adhesive strength is stronger. The bending of the electrode assembly may cause detachment of the electrode and separator at the b side, or may lead to low stiffness of the electrochemical device, which may cause safety issues. When the heat and pressure applied to the electrode assembly are increased to prevent the bending of the electrode assembly, the separator located on the periphery of the electrode assembly suffers from problems such as reduced air permeability and increased electrical resistance due to excessive compression.

[0008] The purpose of the present invention is to provide a zigzag-shaped electrode assembly having a layout structure determined by taking into account the characteristics according to the double-sided coating of the separator and the electrode, and a method for manufacturing the same.

[0009] One aspect of the present invention provides an electrode assembly including a separator bent in a zigzag shape, a cathode disposed between first surfaces of the separator, and an anode disposed between second surfaces of the separator, wherein the anode and the cathode each have an upper surface and a lower surface having a lower adhesive strength than the upper surface, and the upper surface of the anode is disposed to face the upper surface of the cathode with the separator interposed therebetween.

[0010] The upper surface and the lower surface may be active material layers arranged to face each other with the collector interposed therebetween.

[0011] The upper surface may be thicker than the lower surface.

[0012] The upper surface and the lower surface include an active material, a conductive material, and a binder resin, and the upper surface may have a higher content of binder resin than the lower surface.

[0013] The first side of the separator may have a higher surface adhesiveness than the second side.

[0014] The adhesive force between the upper surface of the cathode and the first surface of the separator may be 0.8 to 1.2 times the adhesive force between the upper surface of the anode and the second surface of the separator.

[0015] The adhesive force between the upper surface of the cathode and the first surface of the separator may be 1.5 to 2.5 times the adhesive force between the lower surface of the cathode and the first surface of the separator.

[0016] The above electrode assembly may include n positive electrodes (n is a natural number from 1 to 60) and n+1 negative electrodes.

[0017] The above separation membrane includes a porous substrate, a first porous coating layer formed on one surface of the porous substrate, and a second porous coating layer formed on the other surface of the porous substrate, wherein the first surface may be a surface of the first porous coating layer, and the second surface may be a surface of the second porous coating layer.

[0018] The above porous coating layer includes inorganic particles and a polymer binder, and the first porous coating layer may have a higher content of the polymer binder than the second porous coating layer.

[0019] The electrode assembly may have a long side length of 1.8 to 6.0 times the short side length.

[0020] The thickness of the electrode assembly may be 8 to 20 mm.

[0021] Another aspect of the present invention provides an electrochemical device including the electrode assembly.

[0022] The above electrochemical device may be a lithium secondary battery.

[0023] The zigzag electrode assembly of the present invention maintains the advantage of excellent productivity, while providing a structure in which bending due to the difference in the adhesive strength of electrodes bonded to both sides of a separator is reduced, thereby improving the safety of an electrochemical device including the electrode assembly.

[0024] Figure 1 is a front view of a conventional electrode assembly.

[0025] Figure 2 is a front view of an electrode assembly according to one specific example of the present invention.

[0026] Figure 3 is a front view of an electrode assembly according to one specific example of the present invention.

[0027] Figure 4 is a conceptual diagram showing a process for evaluating the degree of bending of a secondary battery in an experimental example of the present invention.

[0028] Hereinafter, each component of the present invention will be described in more detail so that a person having ordinary skill in the art to which the present invention pertains can easily practice it; however, this is only an example, and the scope of the rights of the present invention is not limited by the following contents.

[0029] The term "comprises" as used herein is used to list materials, compositions, devices, and methods useful in the present invention, but is not limited to the listed examples.

[0030] As used herein, the terms "about" and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values ​​provided to aid understanding of the present invention.

[0031] As used herein, “electrochemical device” may refer to a primary battery, a secondary battery, a super capacitor, etc.

[0032] Hereinafter, specific embodiments of the present invention will be described in detail with reference to the attached drawings. Details in the drawings may be exaggerated, omitted, or schematically illustrated to explain or emphasize the contents of specific embodiments of the present invention.

[0033]

[0034] Figure 2 is a front view of an electrode assembly (2) according to one specific example of the present invention.

[0035] Referring to FIG. 2, one specific example of the present invention provides an electrode assembly (2) including a separator (30) bent in a zigzag shape, a cathode (10) disposed between a first surface of the separator (30), and an anode (20) disposed between a second surface of the separator (30), wherein the anode (20) and the cathode (10) each have an upper surface (11, 21) and a lower surface (12, 22) having a lower adhesive force than the upper surfaces (11, 21), and the upper surface (21) of the anode is disposed to face the upper surface (11) of the cathode with the separator (30) interposed therebetween.

[0036] Although not shown, the separator (30) includes a porous substrate, a first porous coating layer formed on one surface of the porous substrate, and a second porous coating layer formed on the other surface of the porous substrate. The separator (30) may be folded at predetermined intervals, and a plurality of positive electrodes (20) and negative electrodes (10) may be alternately arranged therebetween. Preferably, the intervals may all be the same.

[0037] The porous substrate may be a porous membrane having a plurality of pores formed therein, which electrically insulates the positive electrode (20) and the negative electrode (10) to prevent a short circuit. For example, when the electrochemical device is a lithium secondary battery, the porous substrate may be an ion-conductive barrier that blocks electrical contact between the positive electrode (20) and the negative electrode (10) while allowing lithium ions to pass therethrough. At least a portion of the pores may form a three-dimensional network that connects the surface and the interior of the porous substrate, and a fluid may pass through the porous substrate through the pores.

[0038] The porous substrate may use a material that is physically and chemically stable with respect to the organic solvent electrolyte. For example, the porous substrate may include, but is not limited to, a resin such as a polyolefin-based resin such as polyethylene, polypropylene, and polybutylene, polyvinyl chloride, polyethylene terephthalate, polycycloolefin, polyethersulfone, polyamide, polyimide, polyimideamide, nylon, polytetrafluoroethylene, and copolymers or mixtures thereof. A polyolefin-based resin may be preferably used. A polyolefin-based resin is suitable for manufacturing an electrochemical device with a higher energy density because it can be processed into a relatively thin thickness and the application of a coating slurry is easy.

[0039] The porous substrate may have a single-layer or multi-layer structure. The porous substrate may include two or more polymer resin layers having different melting points (Tm), thereby providing a shutdown function in the event of a high-temperature runaway of the battery. For example, the porous substrate may include a polypropylene layer having a relatively high melting point and a polyethylene layer having a relatively low melting point. Preferably, the porous substrate may have a three-layer structure in which polypropylene, polyethylene, and polypropylene are laminated in that order. The polyethylene layer melts when the temperature of the battery rises above a predetermined temperature, thereby shutting down the pores, thereby preventing thermal runaway of the battery.

[0040] The thickness of the porous substrate may be 1 ㎛ or more and 100 ㎛ or less. Specifically, the thickness of the porous substrate may be 10 ㎛ or more and 90 ㎛ or less, 20 ㎛ or more and 80 ㎛ or less, 30 ㎛ or more and 70 ㎛ or less, or 40 ㎛ or more and 60 ㎛ or less. Preferably, the thickness of the polymer substrate may be 1 ㎛ or more and 30 ㎛ or less. More preferably, the thickness of the polymer substrate may be 5 ㎛ or more and 15 ㎛ or less, or 7 ㎛ or more and 13 ㎛ or less. By controlling the thickness of the porous substrate within the above-described range, the volume of the electrochemical device can be minimized while electrically insulating the positive and negative electrodes, thereby increasing the amount of active material included in the electrochemical device.

[0041] The porous substrate may include pores having an average diameter of 0.01 μm or more and 1 μm or less. Specifically, the size of the pores included in the porous substrate may be 0.01 μm or more and 0.09 μm or less, 0.02 μm or more and 0.08 μm or less, 0.03 μm or more and 0.07 μm or less, or 0.04 μm or more and 0.06 μm or less. Preferably, the size of the pores may be 0.02 μm or more and 0.06 μm or less. By controlling the pore size of the porous substrate within the above-described range, the air permeability and ionic conductivity of the entire manufactured membrane can be controlled.

[0042] The porous substrate may have a permeability of 10 s / 100cc or more and 100 s / 100cc or less. Specifically, the permeability of the porous substrate may be 10 s / 100cc or more and 90 s / 100cc or less, 20 s / 100cc or more and 80 s / 100cc or less, 30 s / 100cc or more and 70 s / 100cc or less, or 40 s / 100cc or more and 60 s / 100cc or less. Preferably, the permeability of the porous substrate may be 50 s / 100cc or more and 70 s / 100cc or less. When the permeability of the porous substrate is within the above-described range, the permeability of the manufactured separator may be provided within a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0043] The above air permeability (s / 100cc) means the time (in seconds) it takes for 100cc of air to pass through a porous substrate or membrane of a predetermined area under a constant pressure. The air permeability can be measured using a Gurley densometer according to ASTM D 726-58, ASTM D726-94 or JIS-P8117. For example, using a 4110N device from Gurley, air at a pressure of 0.304kPa or 1.215 kN / m 2 100 cc of air under the pressure of water occupies 1 square inch (or 6.54 cm 2 ) can be used to measure the time it takes for 100 cc of air to pass through a 1-square-inch sample under a constant pressure of 4.8 inches of water at room temperature. For example, using the Asahi Seico EG01-55-1MR equipment, the time it takes for 100 cc of air to pass through a 1-square-inch sample can be measured.

[0044] The porous substrate may have a porosity of 10 vol% or more and 60 vol% or less. Specifically, the porosity of the porous substrate may be 15 vol% or more and 55 vol% or less, 20 vol% or more and 50 vol% or less, 25 vol% or more and 45 vol% or less, or 30 vol% or more and 40 vol% or less. Preferably, the porosity of the porous substrate may be 30 vol% or more and 50 vol% or less. When the porosity of the porous substrate is in the above-described range, the ionic conductivity of the manufactured separator can be provided in a range suitable for securing the output and cycle characteristics of the electrochemical device.

[0045] The above porosity refers to the volume ratio of pores to the total volume of the porous substrate. The porosity can be measured by methods known in the art. For example, it can be measured by the BET (Brunauer Emmett Teller) measurement method using nitrogen gas adsorption, capillary flow porosimetry, or water or mercury intrusion method.

[0046] The above porous coating layer is formed on at least one surface of the porous substrate, and may include inorganic particles and a polymer binder. Specifically, the porous coating layer may encompass a first porous coating layer and a second porous coating layer. The electrode assembly (2) of the present specific example may use a separator in which a first porous coating layer is formed on one surface of a porous substrate, and a second porous coating layer is formed on the other surface. The separator (30) may be adhered to the negative electrode (10) through the first porous coating layer, and may be adhered to the positive electrode (20) through the second porous coating layer. The first porous coating layer may have one surface adhered to the porous substrate, and the other surface, the first surface, may be adhered to the negative electrode (10). The second porous coating layer may have one surface adhered to the porous substrate, and the other surface, the second surface, may be adhered to the positive electrode (20). When the above separator (30) is folded in a zigzag pattern and the positive electrode (20) and the negative electrode (10) are arranged, the negative electrode (10) can be arranged between the first surface, which is the surface of the first porous coating layer, and the positive electrode (20) can be arranged between the second surface, which is the surface of the second porous coating layer.

[0047] The polymer binder can bind the inorganic particles included in the porous coating layer and provide adhesive strength to the porous coating layer. The polymer binder can be selected from an acrylic polymer binder, a fluorine polymer binder, or a combination thereof.

[0048] The above acrylic polymer binder is (meth)acrylic acid, (meth)acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, n-amyl acrylate, isoamyl acrylate, n-ethylhexyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, n-ethylhexyl methacrylate, 2-ethylhexyl methacrylate, hydroxyethyl methacrylate, (meth)acrylonitrile It may include, as a repeating unit, one or more monomers selected from the group consisting of butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, ethyl (meth)acrylate, methyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, n-oxyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, lauryl (meth)acrylate, tetradecyl (meth)acrylate, and pentafluorophenyl acrylate.

[0049] For example, the acrylic polymer binder may include at least one selected from the group consisting of polyacrylic acid, methyl acrylate, ethyl acrylate, isopropyl acrylate, n-butylacrylate, isobutylacrylate, ethylhexylacrylate, methyl methacrylate, styrene-butadiene rubber, nitrile-butadiene rubber, acrylonitrile-butadiene rubber, and acrylonitrile-butadiene-styrene rubber.

[0050] The above fluorinated polymer binder may be polyvinylidene fluoride. For example, the fluorinated polymer binder may be at least one selected from the group consisting of polyvinylidene fluoride, polyhexafluoropropylene, polytetrafluoroethylene, polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinylidene fluoride-trichloroethylene (PVDF-TCE), and polyvinylidene fluoride-chlorotrifluoroethylene (PVDF-CTFE), and more specifically, may be a copolymer including polyvinylidene fluoride.

[0051] The above inorganic particles can be used as electrochemically stable particles. The above inorganic particles can be used in the operating voltage range of the electrochemical device (e.g., Li / Li + There is no particular limitation as long as no oxidation and / or reduction reaction occurs at 0 to 5 V as a standard. In particular, when using inorganic particles having a high dielectric constant as inorganic particles, it can contribute to increasing the degree of dissociation of electrolyte salt, such as lithium salt, in the liquid electrolyte, thereby improving the ionic conductivity of the electrolyte. For the reasons described above, it is preferable that the inorganic particles include high-dielectric constant inorganic particles having a dielectric constant of 5 or more, preferably 10 or more. Non-limiting examples of inorganic particles having a dielectric constant of 5 or more include BaTiO3, Pb(Zr,Ti)O3(PZT), b 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, Al(OH)3, SiC, AlOOH, TiO2 or mixtures thereof.

[0052] In addition, inorganic particles having lithium ion transfer capability, i.e., inorganic particles containing lithium element but having the function of transferring lithium ions without storing lithium, can be used. Non-limiting examples of inorganic particles having lithium ion transfer capability include lithium phosphate (Li3PO4), lithium titanium phosphate (Li). x Ti y (PO4)3, 0 < x <2, 0 < y <3), lithium aluminum titanium phosphate (Li x Al y Ti z (PO4)3, 0 < x < 2, 0 < y < 1, 0 < z < 3), 14Li2O-9Al2O3-38TiO2-39P2O5, etc. (LiAlTiP) x O y Series glass (0 <x < 4, 0 < y < 13), 리튬란탄티타네이트(Li x La y TiO3, 0 < x <2, 0 <y <3), Li 3.25 Ge 0.25 P 0.75 Lithium germanium thiophosphate (Li) such as S4 x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5), lithium nitride (Li 3 N ), etc. x N y , 0 < x <4, 0 < y < 2), SiS2 series glass (Li) such as Li3PO4-Li2S-SiS2 x Si y S z, 0 < x < 3, 0 <y < 2, 0 < z < 4), LiI-Li2S-P2S5등과 같은 P2S5계열 glass(Li x P y S z , 0 < x < 3, 0< y < 3, 0 < z < 7) or mixtures thereof.

[0053] In addition, as the inorganic particles, inorganic particles having flame retardancy can be used to impart flame retardant properties to the separator or to prevent a rapid increase in temperature inside the electrochemical device. Non-limiting examples of inorganic particles having flame retardancy include Sb2O3, Sb2O4, Sb2O5, SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, Zn2SnO4, ZnSnO3, ZnSn(OH)6, ZrO2, Y2O3, SiO2, Al2O3, AlOOH, Al(OH)3, SiC, TiO2, H3BO3, HBO2, and mixtures thereof.

[0054] The average particle diameter (D50) of the above-mentioned inorganic particles may be 10 nm or more and 10,000 nm or less. Specifically, the average particle diameter (D50) of the above-mentioned inorganic particles may be 100 nm or more and 9,000 nm or less, 1,000 nm or more and 8,000 nm or less, 2,000 nm or more and 7,000 nm or less, 3,000 nm or more and 6,000 nm or less, or 4,000 nm or more and 5,000 nm or less. Preferably, the average particle diameter of the above-mentioned inorganic particles may be 100 nm or more and 700 nm or less. If the average particle diameter of the above-mentioned inorganic particles is less than 10 nm, as the specific surface area increases, an additional polymer binder for bonding between the inorganic particles is required, which is disadvantageous in terms of electrical resistance. If the average particle size of the inorganic particles exceeds 10,000 nm, the uniformity of the coating layer surface may be reduced and damage to the porous substrate or electrode may occur during lamination.

[0055] The above porous coating layer may include a polymer binder and inorganic particles in a weight ratio of 20:80 to 80:20. By controlling the content of the polymer binder and the inorganic particles within the above-described range, thermal shrinkage of the porous substrate can be prevented, thereby preventing electrode short-circuiting due to shrinkage of the separator, and securing adhesion of the separator to the electrode. Specifically, the first porous coating layer may have a higher content of the polymer binder than the second porous coating layer. The first surface of the first porous coating layer may have higher adhesion to the electrode than the second surface of the second porous coating layer.

[0056] The porous coating layer may be formed by coating one surface of the porous substrate with a coating slurry containing the polymer binder, the inorganic particles, and a dispersion medium. The first porous coating layer and the second porous coating layer may contain the same or different polymer binders or inorganic particles. The separator may be manufactured by applying a first coating slurry for forming a first porous coating layer on one surface of the porous substrate and a second coating slurry for forming a second porous coating layer on the other surface, respectively, and drying to remove the dispersion medium. Preferably, the first coating slurry and the second coating slurry may be applied and dried simultaneously. The porous coating layer may have a porous structure including an interstitial volume in which the inorganic particles are connected by a polymer binder. The porous coating layer may allow lithium ions to pass therethrough and may be adhered to the porous substrate to prevent thermal shrinkage of the porous substrate.

[0057] The above coating slurry can dissolve or disperse at least a portion of the polymer binder, including a dispersion medium, and disperse the inorganic particles. The coating slurry can be used in which the inorganic particles are uniformly dispersed by controlling the type or content of the dispersion medium. For example, the dispersion medium can be one selected from the group consisting of water, ethanol, acetone, isopropyl alcohol (IPA), dimethylacetamide (DMAc), dimethylformamide (DMF), N-methyl-2-pyrrolidone (NMP), acetonitrile, and combinations thereof. Preferably, the dispersion medium can be water. By using the above-described type of dispersion medium, a porous coating layer in which the inorganic particles are uniformly dispersed can be formed.

[0058] The above coating slurry may further include additives such as a dispersant, a surfactant, an antifoaming agent, a flame retardant, and a wetting agent to improve dispersibility and flame retardancy and to improve the uniformity of the porous coating layer formed. For example, the dispersant may include at least one selected from the group consisting of a soluble polyamine, a soluble amine compound, fatty acids, fatty alcohols, sorbitan fatty acid esters, tannic acid, and pyrogallic acid. By using the above-described type of dispersant, the stability of the coating slurry can be improved and the uniformity of the porous coating layer formed with the coating slurry can be secured.

[0059] The additive may be included in an amount of 0 wt% or more and 5 wt% or less based on the total weight of the coating slurry. Specifically, the content of the additive may be included in an amount of 0.01 wt% or more and 4 wt% or less, 0.1 wt% or more and 3 wt% or less, or 1 wt% or more and 2 wt% or less. Preferably, the content of the additive may be 3 wt% or more and 5 wt% or less. By controlling the content of the additive within the above-described range, uniform dispersion and stability of the inorganic particles included in the coating slurry can be achieved.

[0060] The dispersion medium included in the coating slurry may be removed by drying or heating after the porous coating layer is formed. For example, the porous coating layer may contain the dispersion medium in an amount of 5 ppm or less. Preferably, the porous coating layer may be composed of a polymer binder and inorganic particles. In the process of removing the dispersion medium, a plurality of pores may be formed on the surface and inside of the porous coating layer. The pores may include interstitial volumes formed between inorganic particles, and may have a structure that allows fluid to pass through by forming a three-dimensional network.

[0061] The thickness of the porous coating layer may be 1 ㎛ or more and 15 ㎛ or less. Specifically, the thickness of the porous coating layer may be 2 ㎛ or more and 14 ㎛ or less, 3 ㎛ or more and 13 ㎛ or less, 4 ㎛ or more and 12 ㎛ or less, 5 ㎛ or more and 11 ㎛ or less, 6 ㎛ or more and 10 ㎛ or less, or 7 ㎛ or more and 9 ㎛ or less. By controlling the thickness of the porous coating layer within the above-described range, shrinkage of the porous substrate can be minimized and stable adhesion to the porous substrate can be implemented. Preferably, the thickness of the first porous coating layer may be thicker than the thickness of the second porous coating layer.

[0062] The separator for the electrochemical device may have a permeability of 50 s / 100cc or more and 300 s / 100cc or less. Specifically, the permeability of the separator may be 100 s / 100cc or more and 250 s / 100cc or less, or 150 s / 100cc or more and 200 s / 100cc or less. Preferably, the permeability of the separator may be 100 s / 100cc or more and 120 s / 100cc or less. When the permeability of the separator is within the above-described range, the output, stability, and cycle characteristics of the electrochemical device can be secured.

[0063] The positive electrode (20) and the negative electrode (10) may be coated by applying and drying an electrode active material on at least one surface of each current collector (23, 13). The current collector may be a material that is conductive and does not cause a chemical change in the electrochemical device. For example, the current collector (23) for the positive electrode may be made of, but is not limited to, aluminum, nickel, titanium, calcined carbon, stainless steel; aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and the like. For example, the current collector (13) for the negative electrode may be made of, but is not limited to, copper, nickel, titanium, calcined carbon, stainless steel; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; and the like. The current collector may be in various forms, such as a metal plate, film, foil, net, porous body, foam, etc.

[0064] The positive electrode (20) has a positive electrode current collector (23) and a positive electrode active material layer (21, 22) including a positive electrode active material, a conductive material, and a binder resin on both sides of the positive electrode current collector (23). Specifically, the positive electrode (20) includes an upper surface (21) formed on one side of the current collector (23) and a lower surface (22) formed on the other side. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M xNi-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x M x A lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a part of the Li in the chemical formula is replaced with an alkaline earth metal ion; a disulfide compound; and Fe2(MoO4)3 may include one or a mixture of two or more thereof. Preferably, the positive electrode active material may include one or more transition metals.

[0065] The negative electrode (10) has a negative electrode current collector (13) and a negative electrode active material layer (11, 12) including a negative electrode active material, a conductive material, and a binder resin on both sides of the current collector (13). Specifically, the negative electrode (10) includes an upper surface (11) formed on one side of the current collector (13) and a lower surface (12) formed on the other side. The negative electrode (10) includes carbon such as lithium metal oxide, non-graphitizable carbon, graphite carbon, etc. as the negative electrode active material; LixFe2O3(0≤x≤1), Li x WO2(0≤x≤1), Si, SiO x (0 <x<2), SiC, Si 합금 등의 실리콘계 재료; Sn x Me 1-x Me' y O z(Me: Mn, Fe, Pb, Ge; Me': Al, B, P, Si, elements of group 1, 2, and 3 of the periodic table, halogens; 0 <x≤1; 1≤y≤3; 1≤z≤8) 등의 금속 복합 산화물; 리튬 금속; 리튬 합금; 주석계 합금; SnO, SnO2, PbO, PbO2, Pb2O3, Pb3O4, Sb2O3, Sb2O4, Sb2O5, GeO, GeO2, Bi2O3, Bi2O4, 및 Bi2O5등의 금속 산화물; 폴리아세틸렌 등의 도전성 고분자; Li-Co-Ni 계 재료; 티타늄 산화물 중 선택된 1종 또는 2종 이상의 혼합물을 포함할 수 있다.

[0066] The conductive material may be one or a mixture of two or more conductive materials selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, carbon nanotubes, activated carbon, and polyphenylene derivatives. The carbon nanotubes have a graphite sheet in the shape of a cylinder with a nano-sized diameter, and sp 2It has a bonding structure, and exhibits the characteristics of a conductor or a semiconductor depending on the angle and structure at which the graphite plane is rolled. Carbon nanotubes can be classified into single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes (DWCNTs), and multi-walled carbon nanotubes (MWCNTs) depending on the number of bonds forming the wall, and these carbon nanotubes can be appropriately selected depending on the use of the dispersion. More specifically, it can be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials among these.

[0067] As the above binder resin, a binder resin commonly used in electrodes of electrochemical devices can be used. Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-cotrichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, and carboxyl methyl cellulose.

[0068] The surface adhesive strength of the upper surface (21) and lower surface (22) of the positive electrode (20) may be higher than the surface adhesive strength of the upper surface (11) and lower surface (12) of the negative electrode (10), respectively. The difference in surface adhesive strength between the electrodes may be determined by at least one of the thickness of each electrode and the type and content of the binder resin. For example, the positive electrode (20) may use a fluorine-based binder resin as the binder resin, and the negative electrode (10) may use an acrylic-based binder resin as the binder resin.

[0069] In the positive electrode (20) and the negative electrode (10), the upper surface (21, 11) of each may have a higher surface adhesive strength than the lower surface (22, 12). The lower surface may have a lower surface adhesive strength than the upper surface, and thus may have a relatively lower adhesive strength with the electrode. The difference in surface adhesive strength between the upper surface (11, 21) and the lower surface (12, 22) may be determined by at least one of the thickness of each layer and the binder resin content. Specifically, the thickness of the upper surface (11, 21) of each electrode may be greater than the thickness of the lower surface (12, 22). Alternatively, the upper surface (11, 21) of each electrode may have a higher binder resin content than the lower surface (12, 22). For example, the adhesive force between the upper surface (11) of the cathode and the first surface of the separator (30) may be 1.5 to 2.5 times the adhesive force between the lower surface (12) of the cathode and the first surface of the separator (30).

[0070] The upper surfaces (21, 11) of the positive electrode (20) and the negative electrode (10) may be arranged to face each other with the separator (30) interposed therebetween. Referring to FIG. 2, the upper surface (11) of the negative electrode (10) may be arranged to contact the first surface of the separator, and the upper surface (21) of the positive electrode (20) may be arranged to contact the second surface opposite the first surface. Specifically, the separator (30) may have an adhesive strength of the first surface higher than that of the second surface, and the surface adhesive strength of the upper surface (11) of the negative electrode may be lower than that of the upper surface (21) of the positive electrode.

[0071] The present specific example is characterized by providing an electrode assembly in which the first surface of the separator (30) is bonded to the cathode (10) and the second surface of the separator (30) is bonded to the anode (20) so that the deviation in electrode-separator adhesive force applied to both surfaces of the separator (30) is not large. The electrode-separator adhesive force (adhesion of surface a) between the upper surface (11) of the cathode and the first surface of the separator (30) may be 0.8 to 1.2 times the electrode-separator adhesive force (adhesion of surface d) between the upper surface (21) of the anode and the second surface of the separator (30). Specifically, the adhesive force between the upper surface (11) of the cathode and the first surface of the separator (30) may be 0.85 to 1.15 times, 0.9 to 1.1 times, or 0.95 to 1.05 times the adhesive force between the upper surface (21) of the anode and the second surface of the separator (30). Preferably, the adhesive force between the upper surface (11) of the cathode and the first surface of the separator (30) may be the same as the adhesive force between the upper surface (21) of the anode and the second surface of the separator (30).

[0072] It will be understood that, according to the arrangement described above, the lower surface (22) of the anode (20) can be arranged to face the lower surface (12) of the cathode (10) with the separator (30) therebetween. The electrode-separator adhesive force (adhesion of side b) between the lower surface (12) of the cathode and the first surface of the separator (30) may be 0.8 to 1.2 times the electrode-separator adhesive force (adhesion of side c) between the lower surface (22) of the anode and the second surface of the separator (30). Specifically, the adhesive force between the lower surface (12) of the cathode and the first surface of the separator (30) may be 0.85 to 1.15 times, 0.9 to 1.1 times, or 0.95 to 1.05 times the adhesive force between the lower surface (22) of the anode and the second surface of the separator (30). Preferably, the adhesive force between the lower surface (12) of the cathode and the first surface of the separator (30) may be the same as the adhesive force between the lower surface (22) of the anode and the second surface of the separator (30).

[0073] As described above, the electrode assembly (2) in which the relative arrangement of each electrode (10, 20) and the separator (30) is determined has a small deviation in the electrode-separator adhesive strength on both sides based on a portion of the separator (30), so that even when a plurality of electrodes are stacked to make the overall thickness of the electrode assembly thicker, bending of the separator (30) may not occur or may be reduced. For example, in the conventional electrode assembly (1) as in Fig. 1, when the number of anodes is approximately 30 or more, bending of the separator (30) may occur or detachment of the electrode may occur as the deviation in the electrode-separator adhesive strength on both sides of the separator (30) increases despite thermal compression of the electrode assembly. The electrode assembly (2) according to this specific example includes n positive electrodes (20) (n is a natural number from 1 to 60) and n+1 negative electrodes (10), and even when a larger number of electrodes are stacked, the electrode-separator adhesive force on both sides of the separator can be maintained in balance, thereby preventing bending and electrode detachment.

[0074] The electrode assembly (2) may have a long side length that is 1.8 to 6.0 times the short side length. The electrode assembly (2) may have a thickness of 8 to 20 mm. The electrode assembly (2) having the dimensions within the above-described range has excellent safety due to bending prevention, and is therefore suitable for storage in an electric vehicle.

[0075] Fig. 3 is a front view of an electrode assembly (3) according to another specific example of the present invention. The same contents as the electrode assembly (2) of Fig. 2 are replaced with the previous specific example.

[0076] Referring to FIG. 3, the electrode assembly (3) may have the stacking directions of the positive electrode (20) and the negative electrode (10) opposite each other compared to the electrode assembly (2) of the preceding specific example. Even in this case, the upper surface (11) of the negative electrode may be arranged to face the upper surface (21) of the positive electrode with the separator (30) interposed therebetween. The electrode-separator adhesive strength (adhesion of the b side) between the upper surface (11) of the negative electrode and the first side of the separator (30) may be 0.8 to 1.2 times the electrode-separator adhesive strength (adhesion of the c side) between the upper surface (21) of the positive electrode and the second side of the separator (30). Specifically, the adhesive force between the upper surface (11) of the cathode and the first surface of the separator (30) may be 0.85 to 1.15 times, 0.9 to 1.1 times, or 0.95 to 1.05 times the adhesive force between the upper surface (21) of the anode and the second surface of the separator (30), and preferably may be the same.

[0077] It will be understood that, according to the arrangement described above, the lower surface (22) of the anode (20) can be arranged to face the lower surface (12) of the cathode (10) with the separator (30) therebetween. The electrode-separator adhesive strength (adhesion of side a) between the lower surface (12) of the cathode and the first surface of the separator (30) may be 0.8 to 1.2 times, preferably equal to, the electrode-separator adhesive strength (adhesion of side d) between the lower surface (22) of the anode and the second surface of the separator (30).

[0078] As described above, the electrode assembly (3) in which the relative arrangement of each electrode (10, 20) and the separator (30) is determined has a small deviation in electrode-separator adhesion on both sides based on a portion of the separator (30), so that even when a plurality of electrodes are stacked to increase the overall thickness of the electrode assembly, bending of the separator (30) can be prevented or reduced.

[0079]

[0080] Another embodiment of the present invention provides an electrochemical device comprising an electrode assembly (2, 3) according to the above-described embodiment. The electrochemical device can be manufactured by inserting and sealing one or more electrode assemblies (2, 3) into a case or pouch. Before sealing the case or pouch, an electrolyte can be injected to impregnate the electrode assembly with the electrolyte. The shape of the case or pouch is not limited. For example, the electrochemical device can be a cylindrical, square, coin-shaped, or pouch-shaped lithium secondary battery.

[0081] The above electrolyte is A + B - As a salt with the same structure, A + is Li + , Na + , K + Contains ions composed of alkali metal cations or combinations thereof, such as B - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 - , AsF6 - , CH3CO2 - , CF3SO3 - , N(CF3SO2)2 - , C(CF2SO2)3 -A salt comprising an anion such as or a combination thereof may be dissolved or dissociated in an organic solvent comprising propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone or a mixture thereof.

[0082] The electrochemical device including the electrode assembly may be a lithium secondary battery. The battery may be used as a unit cell, and may be used as a battery module including the unit cell, a battery pack including the battery module, or a device including the battery pack as a power source. The devices may include, but are not limited to, small devices such as computers, mobile phones, and power tools; electric vehicles including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs) that are powered by an electric motor; electric two-wheeled vehicles including electric bicycles (E-bikes) and electric scooters; electric golf carts; and power storage systems.

[0083]

[0084] Another specific example of the present invention provides a method for manufacturing the electrode assembly (2), comprising the steps of (S10) forming a laminate by zigzag-folding a separator (30) and alternately arranging a positive electrode (20) and a negative electrode (10) therebetween, and (S20) manufacturing the electrode assembly (2) by applying heat and pressure to the laminate. In the description of the method for manufacturing the electrode assembly (2), the same content as the description of the electrode assembly (2) described above is replaced with the description of the preceding specific example.

[0085] The above step (S10) is a step of forming a laminate by alternately arranging a positive electrode (20) and a negative electrode (10) between folds formed by zigzag-folding a separator (30). The length of the separator (30) in the longitudinal direction (or MD direction; Machine Direction) may be longer than the length of the width direction (or TD direction; Transverse Direction). The separator (30) may be folded in a zigzag manner at a predetermined interval along the MD direction. The arrangement of the positive electrode (20) and the negative electrode (10) may be such that the upper surface (21) of the positive electrode and the upper surface (11) of the negative electrode face each other with the separator (30) interposed therebetween. The separator (30) may include a first surface and a second surface having lower surface adhesiveness than the first surface, and the negative electrode (10) may be arranged between the first surface and the positive electrode (20) between the second surface.

[0086] The separator (30), the anode (20), and the cathode (10) may each have a rectangular shape, but are not limited thereto. For example, the separator (30), the anode (20), and the cathode (10) may each have a rectangular shape in which the MD direction is longer than the TD direction. The anode (20) and the cathode (10) may be arranged in multiples along the MD direction of the separator (30), and may be arranged such that the MD direction of the separator (30) and the TD directions of the anode (20) and the cathode (10) are parallel to each other. Preferably, the anode (20) and the cathode (10) may be aligned such that their respective TD direction center lines coincide.

[0087] The above step (S20) is a step of manufacturing an electrode assembly (2) in which a positive electrode (20) and a separator (30) and a negative electrode (10) and a separator (30) are bonded by thermocompression bonding the laminate formed in the above step (S10). The thermocompression bonding may be performed by compressing the uppermost and lowermost ends of the laminate using a press device, and may be performed by applying a pressure of 1 to 7 MPa at a temperature of 45 to 80° C. for 1 to 30 seconds to one or more laminates. By controlling the temperature and pressure conditions of the thermocompression bonding within the above-described range, uniform bonding of the separators (30) and electrodes (10, 20) constituting the laminate can be realized without causing damage to the laminate. The type of the press device is not limited as long as it can bond the separators and electrodes by simultaneously or simultaneously applying heat and pressure to one or both sides of the laminate while maintaining the alignment of the separators and electrodes included in the laminate.

[0088] Preferably, the thermocompression bonding can be divided into two or more steps. The step (S20) may include a first thermocompression bonding for fixing the relative position of the electrodes (10, 20) with respect to the separator (30) by applying a pressure of 1 to 6 MPa at 45 to 65°C for 1 to 30 seconds, and a second thermocompression bonding for completely bonding the separator (30) and the electrodes (10, 20) by applying a pressure of 1 to 7 MPa at 50 to 80°C for 1 to 30 seconds. The first thermocompression bonding may partially bond the electrodes (10, 20) adjacent to the separator (30) to fix the position of the electrodes. The second thermocompression bonding may completely bond the separator (30) and the electrodes (10, 20) at the position determined through the first thermocompression bonding to manufacture the electrode assembly (2). Through the above first thermocompression bonding and the second thermocompression bonding, an electrode assembly (2) can be manufactured in which alignment is superior compared to single-stage thermocompression bonding and electrode-separator adhesion is uniformly formed. Through the above first thermocompression bonding and the second thermocompression bonding, thermocompression conditions are relaxed compared to single-stage thermocompression bonding, thereby preventing damage to the separator (30), thereby achieving superior production efficiency.

[0089]

[0090] Hereinafter, the present invention will be described in more detail through specific examples and experimental examples. The following examples and experimental examples are intended to illustrate the present invention, and the present invention is not limited by the following examples and experimental examples.

[0091] Example 1

[0092] A 15 ㎛ thick separator manufactured by coating a coating slurry containing inorganic particles and a polymer binder on a 9 ㎛ thick polyethylene substrate was prepared, and 30 and 31 pieces of anodes (upper thickness: 60 ㎛, lower thickness: 50 ㎛) measuring 90 mm × 315 mm and 125 ㎛ thick, and cathodes (upper thickness: 75 ㎛, lower thickness: 65 ㎛) measuring 95.5 mm × 320 mm and 150 ㎛ thick, respectively, were prepared. The separators were folded in a zigzag pattern at intervals of 98.5 mm and arranged so that the upper surfaces of the cathodes and the upper surfaces of the anodes faced each other with the separator in between, thereby preparing a laminate. The above laminate was placed on a press device, and thermo-compression was performed at 60°C and a pressure of 6 MPa for 1 second, and then thermo-compression was performed at 70°C and a pressure of 6 MPa for 1 second to manufacture an electrode assembly having a shape as shown in Fig. 2.

[0093] The electrode assembly was placed inside the case using a pouch outer material of a laminated sheet of CPP / aluminum / nylon as a case, an ethyl methyl carbonate (EMC) electrolyte containing LiPF6 was injected, and the pouch outer material was heat-sealed to complete the assembly of the secondary battery.

[0094] Afterwards, the secondary battery was subjected to a pre-activation heating press process and an activation process. The heating press process was performed at a temperature of 30°C and a pressure of 3.0 kgf / cm. 2 It was performed for 5 minutes under pressure conditions. The activation process was performed at a temperature of 50℃ and a pressure of 1.0 kgf / cm 2 The secondary battery was charged at 0.5 C under pressure conditions.

[0095] Example 2

[0096] An electrode assembly and secondary battery having the same shape as in Fig. 3 were manufactured using the same method as Example 1, except that the stacking directions of the positive and negative electrodes were reversed.

[0097] Comparative Example 1

[0098] An electrode assembly and secondary battery having the same shape as in Fig. 1 were manufactured using the same method as Example 1, except that the upper surface of the negative electrode and the lower surface of the positive electrode were arranged to face each other with a separator between them.

[0099] Example 3

[0100] An electrode assembly and a secondary battery were manufactured in the same manner as in Example 1, except that an electrode having a negative electrode with a long side of 525 mm and an anode with a long side of 520 mm was used.

[0101] Comparative Example 2

[0102] An electrode assembly and a secondary battery were manufactured in the same manner as in Comparative Example 1, except that an electrode having a long side of the cathode of 525 mm and a long side of the anode of 520 mm was used.

[0103] Comparative Example 3

[0104] An electrode assembly and a secondary battery were manufactured in the same manner as in Comparative Example 1, except that 68 and 69 positive and negative electrodes were used, respectively.

[0105] Comparative Example 4

[0106] An electrode assembly and a secondary battery were manufactured in the same manner as in Comparative Example 1, except that an electrode having a long side of the cathode of 605 mm and a long side of the anode of 600 mm was used.

[0107] Experimental example

[0108] Confirming the adhesion of the electrode-separator

[0109] With reference to Figures 1 to 3, the electrode-separator adhesion on planes a to d of the electrode assemblies manufactured in the examples and comparative examples was confirmed.

[0110] The adhesive strength when peeling the electrode from the separator was measured while peeling the electrode layer by layer at a speed of 90° and 200 mm / min on each electrode assembly surface a to d, and the results are summarized in Table 1 below.

[0111] Checking the bending of secondary batteries

[0112] Referring to Fig. 4, a method for evaluating the bending level of a secondary battery is described. The secondary battery (100) including the electrode assembly of the examples and comparative examples that have completed the activation process may have a shape in which one side is concavely bent. As shown in Fig. 2, the secondary battery (100) was placed on a flat surface (G) with the concave side facing upward. A first ruler (A) was placed at both ends of the concave side, and a second ruler (B) was placed in a direction perpendicular to the first ruler (A), and the longest distance (d, mm) between the secondary battery (100) and the first ruler (A) was evaluated as the bending level, which is shown in the table below. The bending level of the secondary battery can be evaluated as good when it is less than 5 mm.

[0113] Example 1 Example 2 Comparative Example 1 Example 3 Comparative Example 2 Comparative Example 3 Comparative Example 4 Number of electrodes (anode / cathode) 30 / 3130 / 3130 / 3130 / 3130 / 3168 / 69 30 / 31 Thickness of electrode assembly (mm) 9.39.39.39.39.320.99.3 Long side / short side ratio of electrode assembly 3.3 3.33.35.45.43.36.3 Adhesion of electrode-separator (gf / 25mm) a 10 5 10 10 10 10 10 b 5 10 5 5 5 5 c 5 10 10 5 10 10 10 d 10 5 10 5 5 5 Occurrence of bending × × ○ × ○ ○ ○ Bending level (mm) 2 3 10 3 11 13 12

[0114]

[0115] [Explanation of symbols]

[0116] 1, 2, 3: Electrode assembly

[0117] 10: Cathode 11: Top surface of the cathode

[0118] 12: Lower surface of the cathode 13: Current collector of the cathode

[0119] 20: Anode 21: Top surface of anode

[0120] 22: Bottom of the positive electrode 23: Current collector of the positive electrode

[0121] 30: Membrane

[0122] 100: Secondary battery

[0123] A: First party B: Second party

Claims

1. A separator that is folded in a zigzag shape; A cathode disposed between the first surfaces of the above separator; and An electrode assembly including an anode disposed between the second surfaces of the separator, The above anode and the above cathode each have an upper surface and a lower surface with lower adhesive strength than the upper surface, An electrode assembly in which the upper surface of the positive electrode is positioned to face the upper surface of the negative electrode with the separator interposed therebetween.

2. In paragraph 1, An electrode assembly in which the upper surface and the lower surface are active material layers arranged to face each other with a current collector interposed therebetween.

3. In paragraph 1, An electrode assembly wherein the upper surface is thicker than the lower surface.

4. In paragraph 1, The upper surface and the lower surface include an active material, a conductive material, and a binder resin, An electrode assembly wherein the upper surface has a higher binder resin content than the lower surface.

5. In paragraph 1, An electrode assembly, wherein the first side of the separator has a higher surface adhesion than the second side.

6. In paragraph 1, An electrode assembly, wherein the adhesive force between the upper surface of the cathode and the first surface of the separator is 0.8 to 1.2 times the adhesive force between the upper surface of the anode and the second surface of the separator.

7. In paragraph 1, An electrode assembly, wherein the adhesive force between the upper surface of the cathode and the first surface of the separator is 1.5 to 2.5 times the adhesive force between the lower surface of the cathode and the first surface of the separator.

8. In paragraph 1, An electrode assembly comprising n positive electrodes (n is a natural number from 1 to 60) and n+1 negative electrodes.

9. In paragraph 1, The above separator comprises a porous substrate, a first porous coating layer formed on one surface of the porous substrate, and a second porous coating layer formed on the other surface of the porous substrate. An electrode assembly, wherein the first surface is a surface of the first porous coating layer, and the second surface is a surface of the second porous coating layer.

10. In paragraph 9, The above porous coating layer includes inorganic particles and a polymer binder, An electrode assembly, wherein the first porous coating layer has a higher polymer binder content than the second porous coating layer.

11. In paragraph 1, The electrode assembly is an electrode assembly in which the length of the long side is 1.8 to 6.0 times the length of the short side.

12. In paragraph 1, An electrode assembly having a thickness of 8 to 20 mm.

Citation Information

Patent Citations

  • An electrode assembly and a method of manufacturing the same

    KR1020240160355A

  • Electrode assembly

    KR1020160059688A

  • A operating method of a terminal in a wireless communication system and the terminal

    KR1020200063950A

  • a manufacturing method of pellicle frame

    KR102495880B1

  • High speed motor

    KR102766283B1

Cited By

  • Secondary battery and method for manufacturing same

    WO2026215752A1