Nanometric lamellar elemental phosphorus flame retardant for polymeric flame-retardant material, and preparation method therefor and use thereof

By reacting elemental phosphorus with organic amine at high temperature, the nano-layered elemental phosphorus flame retardant is solved, and the problem of large amount of traditional red phosphorus flame retardant is achieved, which is highly efficient, low-toxic and halogen-free flame retardant. Performance, suitable for polymer materials, in line with the development trend of green and environmental protection.

WO2024230197A1PCT designated stage expired Publication Date: 2024-11-14SHENZHEN INST OF ADVANCED TECH CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/142453
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2023-12-27
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The use of traditional red phosphorus flame retardants in polymer materials has problems such as large amounts of use and uneven dispersion and poor compatibility with substrates. In addition, halogen flame retardants have been gradually eliminated due to the release of toxic gases during combustion and need to be developed. Nano-inorganic phosphorus-based flame retardant with excellent performance is replaced.

Method used

By mixing single phosphorus with organic amines evenly, reacting at 120~300°C, centrifugal separation, washing and drying with ethanol, nano-layered single phosphorus flame retardant is prepared, and evenly dispersed in polymer materials to form a sheet-like structure , achieve high flame retardant efficiency and low additive amount.

Benefits of technology

It has achieved high-efficiency flame retardant performance, low smoke, low toxicity and halogen-free nano-layered elemental phosphorus flame retardant, which is uniformly dispersed in polymer materials, overcoming the large amount of traditional red phosphorus flame retardant used and uneven dispersion problems. In line with the development trend of green, environmental protection and efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023142453_14112024_PF_FP_ABST
    Figure CN2023142453_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a nanometric lamellar elemental phosphorus flame retardant for a polymeric flame-retardant material, and a preparation method therefor and a use thereof. The lamella thickness of the nanometric lamellar elemental phosphorus flame retardant is 2-100 nm, and the plane diameter is 20-1000 nm. The preparation method is simple and convenient. The nanometric lamellar elemental phosphorus flame retardant is prepared by activating elemental phosphorus by using organic amine, to generate a P-N bond, and then carrying out P-N bond breakage and P-P bond reorganization at high temperature, wherein the amine can be recycled. The nanometric lamellar elemental phosphorus flame retardant has the advantages of having high flame retardancy efficiency, low addition amount, low smoke, and low toxicity, being halogen-free, etc., effectively overcomes the defects of conventional red phosphorus flame retardants, such as large use amount, non-uniform dispersion, and poor compatibility with a base material, and conforms to the development trend that flame retardants are green, environment-friendly, and efficient.
Need to check novelty before this filing date? Find Prior Art

Description

A nano-layered elemental phosphorus flame retardant for polymer flame retardant materials and its preparation method and application Technical Field

[0001] The present invention belongs to the field of flame retardant materials, and in particular relates to a nano-layered elemental phosphorus flame retardant for polymer flame retardant materials, and a preparation method and application thereof. Background Art

[0002] Polymer materials are widely used in building products, wires and cables, textiles, electronic devices, etc. However, they are generally flammable. Therefore, polymer materials need to be flame-retarded, usually by adding flame retardants.

[0003] Flame retardants are classified according to the flame retardant element, including halogen, phosphorus, nitrogen, silicon, and boron. Halogen-based flame retardants have been gradually phased out in recent years due to the release of large amounts of toxic gases upon combustion. As an alternative, phosphorus-based flame retardants not only overcome the shortcomings of halogen-based flame retardants, such as high smoke production and the release of toxic and corrosive gases during combustion, but also offer excellent flame retardant properties, low smoke levels, low toxicity, and no corrosive gases. Due to their long-lasting flame retardancy, good thermal stability, non-volatility, and halogen-free properties, inorganic phosphorus-based flame retardants are becoming increasingly popular, with red phosphorus being the most widely researched. However, traditional red phosphorus flame retardants have drawbacks such as large usage amounts, uneven dispersion, and poor compatibility with substrates.

[0004] Inorganic nanoparticles have recently attracted increasing attention as a new type of flame retardant. This is attributed to the fact that the addition of a small amount of nanoparticles can significantly reduce the heat release rate and mass loss rate of polymer materials. The geometric characteristics of nanoparticles largely determine their flame retardant properties. Nanoparticles with layered structures have been reported to exhibit superior flame retardancy compared to particles with tubular or spherical structures. Therefore, the development of high-performance nano-inorganic phosphorus-based flame retardants is of great significance.

[0005] Summary of the Invention

[0006] The present invention aims to provide a nano-layered elemental phosphorus flame retardant for polymer flame retardant materials, as well as its preparation method and application. The developed nano-layered elemental phosphorus flame retardant has the advantages of high flame retardant efficiency, low addition amount, low smoke, low toxicity, and halogen-free.

[0007] The technical solution of the present invention is:

[0008] A method for preparing a nano-layered elemental phosphorus flame retardant for polymer flame retardant materials, the preparation steps are as follows:

[0009] The elemental phosphorus and the organic amine are uniformly mixed, reacted at 120-300°C for 3-48 hours, centrifuged, washed with ethanol, and dried to a constant weight to obtain a nano-layered elemental phosphorus flame retardant.

[0010] Preferably, the ratio of elemental phosphorus to organic amine is 0.01-2 g:1 mL.

[0011] Preferably, the elemental phosphorus is selected from at least one of white phosphorus, amorphous red phosphorus, black phosphorus, purple phosphorus, and fibrous phosphorus.

[0012] Preferably, the organic amine is selected from at least one of N-methylethylenediamine, N-ethylethylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, 3-dimethylaminopropylamine, 3-methylaminopropylamine, N,N'-bis(3-aminopropyl)ethylenediamine, 3,3'-diaminodipropylamine, N,N'-bis(3-aminopropyl)methylamine, n-octylamine, n-hexylamine, n-butylamine, and 1,2-cyclohexanediamine.

[0013] Preferably, the nano-layered elemental phosphorus flame retardant has a sheet structure with a sheet thickness of 2 to 100 nm and a plane diameter of 20 to 1000 nm.

[0014] The invention also provides a nano-layered elemental phosphorus flame retardant prepared by the preparation method.

[0015] The present invention also provides the use of the nano-layered elemental phosphorus flame retardant prepared by the preparation method in the preparation of polymer flame retardant materials.

[0016] Preferably, the preparation method of the polymer flame retardant material is:

[0017] The polymer material is first heated and melted, and then the nano-layered elemental phosphorus flame retardant is added, stirred evenly and pressed into shape; or the nano-layered elemental phosphorus flame retardant is first added before the monomer of the polymer material is polymerized, and then stirred evenly and polymerized into shape.

[0018] Preferably, the added amount of the nano-layered elemental phosphorus flame retardant accounts for 0.1% to 10% of the mass of the polymer material.

[0019] Preferably, the polymer material is selected from any one of epoxy resin, polyurethane, and ethylene-vinyl acetate copolymer.

[0020] Compared with the prior art, the advantages of the present invention are:

[0021] (1) In the technical solution of the present invention, the nano-layered elemental phosphorus flame retardant is firstly prepared by moderately activating the raw material elemental phosphorus with amine, and then the intermediate undergoes PN bond cleavage at high temperature and then undergoes PP bond recombination. That is, the nano-layered elemental phosphorus flame retardant of the present invention is obtained through the processes of PN bond generation, PN bond cleavage, and PP bond recombination; the amine used can be recycled.

[0022] (2) The nano-layered elemental phosphorus flame retardant of the present invention is a phosphorus element and has the advantages of excellent flame retardancy, low toxicity, and smoke suppression.

[0023] (3) The nano-layered elemental phosphorus flame retardant of the present invention has a layered structure and has an excellent size effect. It can be evenly dispersed in polymer materials and has good compatibility with polymer materials. When added in low amounts, it can achieve high-efficiency flame retardancy, effectively overcoming the shortcomings of traditional red phosphorus flame retardants such as large usage, uneven dispersion, and poor compatibility with substrates, and is in line with the development trend of green, environmentally friendly and efficient flame retardants. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present invention and, together with the description, serve to explain the principles of the invention, in which:

[0025] FIG1 is a scanning electron microscope photograph of the nano-layered elemental phosphorus flame retardant obtained in Example 2 of the present invention;

[0026] FIG2 is an atomic force microscope image of the nano-layered elemental phosphorus flame retardant obtained in Example 2 of the present invention;

[0027] FIG3 is a comparison of the flame retardant properties of the nano-layered elemental phosphorus flame retardant obtained in Example 2 of the present invention and the traditional red phosphorus flame retardant.

[0028] DETAILED DESCRIPTION

[0029] The following disclosure provides many different embodiments or examples for implementing different structures of the present invention. To simplify the disclosure of the present invention, the components and configurations of specific examples are described below. Of course, these are merely examples and are not intended to limit the present invention. In addition, the present invention may repeat reference numbers and / or reference letters in different examples. Such repetition is for the purpose of simplicity and clarity and does not in itself indicate the relationship between the various embodiments and / or configurations discussed.

[0030] Example 1

[0031] Amorphous red phosphorus and N,N'-bis(3-aminopropyl)methylamine were uniformly mixed at a ratio of 0.01 g:1 mL, reacted at 120°C for 48 hours, centrifuged, washed with ethanol, and dried to a constant weight to obtain nano-layered elemental phosphorus flame retardant A. The nano-layered elemental phosphorus flame retardant A had a layer thickness of 100 nm and a planar diameter of 500 nm.

[0032] The polymer material ethylene-vinyl acetate copolymer is heated and melted at 100°C, and a nano-layered elemental phosphorus flame retardant A is added. The mixture is stirred evenly and pressed into shape to obtain a flame-retardant ethylene-vinyl acetate copolymer composite material, which is referred to as flame-retardant polymer material A. The amount of the nano-layered elemental phosphorus flame retardant A added is 10% of the mass of the ethylene-vinyl acetate copolymer.

[0033] Example 2

[0034] Amorphous red phosphorus and N-ethylethylenediamine were uniformly mixed in a ratio of 0.1 g:1 mL, reacted at 220°C for 24 h, centrifuged, washed with ethanol, and dried to a constant weight to obtain a nano-layered elemental phosphorus flame retardant B.

[0035] Figures 1 and 2 are scanning electron microscope photos and atomic force microscope images of the nano-layered elemental phosphorus flame retardant B, respectively. It can be seen that the planar diameter of the nano-layered elemental phosphorus flame retardant B is about 200 nm and the layer thickness is about 15 nm, which confirms the successful preparation of the nano-layered elemental phosphorus material and proves the feasibility of the technical solution of the present invention.

[0036] First, nano-layered elemental phosphorus flame retardant B was mixed with cold-embedded epoxy resin CER1000 (purchased from Guangzhou Weiyi Metallographic Testing Instrument Co., Ltd.) and stirred thoroughly. The mixture was then mixed with epoxy resin curing agent CEH500 (purchased from Guangzhou Weiyi Metallographic Testing Instrument Co., Ltd.) and cured at 60°C. After the curing process, the sample was naturally cooled to room temperature to obtain an epoxy resin composite material, which was calculated as flame-retardant polymer material B. The addition amount of nano-layered elemental phosphorus flame retardant B was 1% of the epoxy resin mass.

[0037] Example 3

[0038] White phosphorus and N-methylethylenediamine were uniformly mixed at a ratio of 2 g:1 mL, reacted at 300°C for 3 h, centrifuged, washed with ethanol, and dried to a constant weight to obtain nano-layered elemental phosphorus flame retardant C. The nano-layered elemental phosphorus flame retardant C had a sheet thickness of 2 nm and a planar diameter of 20 nm.

[0039] First, nano-layered elemental phosphorus flame retardant C was mixed with cold-embedded epoxy resin CER1000, stirred evenly, and then mixed with epoxy resin curing agent CEH500 and cured at 60°C. After the curing process, the sample was naturally cooled to room temperature to obtain an epoxy resin composite material, which was calculated as flame-retardant polymer material C. The addition amount of nano-layered elemental phosphorus flame retardant C was 0.1% by weight of the epoxy resin.

[0040] Example 4

[0041] Black phosphorus and N,N-dimethylethylenediamine were uniformly mixed at a ratio of 1 g:1 mL, reacted at 150°C for 8 h, centrifuged, washed with ethanol, and dried to a constant weight to obtain nano-layered elemental phosphorus flame retardant D. The nano-layered elemental phosphorus flame retardant D had a sheet thickness of 80 nm and a planar diameter of 1000 nm.

[0042] The polymer material polyurethane is heated and melted, and a nano-layered elemental phosphorus flame retardant D is added. The mixture is stirred evenly and pressed into shape to obtain a flame-retardant ethylene-vinyl acetate copolymer composite material, which is referred to as the flame-retardant polymer material D. The amount of the nano-layered elemental phosphorus flame retardant D added is 5% by mass of the ethylene-vinyl acetate copolymer.

[0043] Example 5

[0044] Purple phosphorus and N,N-diethylethylenediamine were uniformly mixed at a ratio of 0.5 g:1 mL, reacted at 180°C for 30 h, centrifuged, washed with ethanol, and dried to a constant weight to obtain nano-layered elemental phosphorus flame retardant E. The nano-layered elemental phosphorus flame retardant E had a layer thickness of 20 nm and a planar diameter of 400 nm.

[0045] First, nano-layered elemental phosphorus flame retardant E was mixed with cold-embedded epoxy resin CER1000, stirred evenly, and then mixed with epoxy resin curing agent CEH500. The mixture was cured at 60°C. After the curing process, the sample was naturally cooled to room temperature to obtain an epoxy resin composite material, which was calculated as flame-retardant polymer material E. The addition amount of nano-layered elemental phosphorus flame retardant E was 2% of the epoxy resin mass.

[0046] Example 6

[0047] Cellulose phosphorus and N,N-diethylethylenediamine / 3-methylaminopropylamine were uniformly mixed in a ratio of 0.2 g:0.5 mL:0.5 mL, and reacted at 250°C for 18 hours. The mixture was centrifuged, washed with ethanol, and dried to a constant weight to obtain a nano-layered elemental phosphorus flame retardant F. The nano-layered elemental phosphorus flame retardant F had a sheet thickness of 10 nm and a planar diameter of 100 nm.

[0048] The polymer material ethylene-vinyl acetate copolymer is heated and melted at 100°C, and a nano-layered elemental phosphorus flame retardant F is added. The mixture is stirred evenly and pressed into shape to obtain a flame-retardant ethylene-vinyl acetate copolymer composite material, which is referred to as the flame-retardant polymer material F. The amount of the nano-layered elemental phosphorus flame retardant F added is 5% of the mass of the ethylene-vinyl acetate copolymer.

[0049] Example 7

[0050] White phosphorus / amorphous red phosphorus and N-ethylethylenediamine were uniformly mixed in a ratio of 0.1 g:0.4 g:1 mL. The mixture was reacted at 200°C for 15 hours, centrifuged, washed with ethanol, and dried to a constant weight to obtain nano-layered elemental phosphorus flame retardant G. The nano-layered elemental phosphorus flame retardant G had a sheet thickness of 40 nm and a planar diameter of 600 nm.

[0051] First, nano-layered elemental phosphorus flame retardant G was mixed with cold-embedded epoxy resin CER1000, stirred evenly, and then mixed with epoxy resin curing agent CEH500 and cured at 60°C. After the curing process, the sample was naturally cooled to room temperature to obtain an epoxy resin composite material, which was calculated as flame-retardant polymer material G. The addition amount of nano-layered elemental phosphorus flame retardant G was 8% of the epoxy resin mass.

[0052] Examples 8-15

[0053] The organic amine in Example 2 was replaced with the organic amine in Table 1, and other experimental conditions remained unchanged. The obtained nano-layered elemental phosphorus flame retardant was tested by scanning electron microscopy and atomic force microscopy to determine its plane diameter and layer thickness (statistical results). The test results are shown in Table 1.

[0054] Table 1 Planar diameter and sheet thickness of the organic amines used in Examples 8 to 15 and the resulting nano-layered elemental phosphorus flame retardants

[0055] Example Organic amine Plane diameter (nm) Layer thickness (nm) Example 8 3-dimethylaminopropylamine 87090 Example 9 3-methylaminopropylamine 62040 Example 10 N,N'-bis(3-aminopropyl)ethylenediamine 9506 Example 11 3,3'-diaminodipropylamine 18010 Example 12 n-octylamine 908 Example 13 n-hexylamine 70085 Example 14 n-butylamine 6020 Example 15 1,2-cyclohexanediamine 44065

[0056] Comparative Example

[0057] First, a traditional red phosphorus flame retardant, AT-88 (purchased from Suzhou Antfeld New Materials Co., Ltd.), was mixed with a cold-embedded epoxy resin, CER1000, and stirred thoroughly. The mixture was then mixed with an epoxy resin curing agent, CEH500, and cured at 60°C. After the curing process, the sample was naturally cooled to room temperature to obtain an epoxy resin composite material, which was used as a comparative flame-retardant polymer material. The traditional red phosphorus flame retardant was added at a concentration of 1% by weight of the epoxy resin.

[0058] The flame retardant properties of the nano-layered elemental phosphorus flame retardant B obtained in Example 2 of the present invention and the traditional red phosphorus flame retardant of the comparative example were evaluated by cone calorimetry. As shown in Figure 3, the flame retardant properties of the nano-layered elemental phosphorus flame retardant B of the present invention are significantly better than those of the traditional red phosphorus flame retardant, and the application prospects are good.

[0059] Other embodiments of the present invention will readily occur to those skilled in the art upon consideration of the specification and practice of the invention herein. The present invention is intended to cover any variations, uses, or adaptations of the present invention that follow the general principles of the invention and include common knowledge or customary techniques in the art. The description and examples are to be considered as exemplary only, with the true scope and spirit of the invention being indicated by the claims.

[0060] It should be understood that the present invention is not limited to the exact construction described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present invention is limited only by the appended claims.

Claims

1. A method for preparing a nano-layered elemental phosphorus flame retardant for polymer flame retardant materials, characterized in that: The preparation steps are as follows: The elemental phosphorus and the organic amine are uniformly mixed, reacted at 120-300° C. for 3-48 h, centrifuged, washed with ethanol, and dried to a constant weight to obtain the nano-layered elemental phosphorus flame retardant.

2. The method for preparing the nano-layered elemental phosphorus flame retardant for polymer flame retardant materials according to claim 1, characterized in that: The ratio of the elemental phosphorus to the organic amine is 0.01-2 g:1 mL.

3. The method for preparing the nano-layered elemental phosphorus flame retardant for polymer flame retardant materials according to claim 1, characterized in that: The elemental phosphorus is selected from at least one of white phosphorus, amorphous red phosphorus, black phosphorus, purple phosphorus and fibrous phosphorus.

4. The method for preparing the nano-layered elemental phosphorus flame retardant for polymer flame retardant materials according to claim 1, characterized in that: The organic amine is selected from at least one of N-methylethylenediamine, N-ethylethylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, 3-dimethylaminopropylamine, 3-methylaminopropylamine, N,N'-bis(3-aminopropyl)ethylenediamine, 3,3'-diaminodipropylamine, N,N'-bis(3-aminopropyl)methylamine, n-octylamine, n-hexylamine, n-butylamine, and 1,2-cyclohexanediamine.

5. The method for preparing the nano-layered elemental phosphorus flame retardant for polymer flame retardant materials according to claim 1, characterized in that: The nano-layered elemental phosphorus flame retardant is a flake structure, the thickness of the flake is 2-100 nm, and the plane diameter is 20-1000 nm.

6. The nano-layered elemental phosphorus flame retardant prepared by the preparation method according to any one of claims 1 to 5.

7. Use of the nano-layered elemental phosphorus flame retardant prepared by the preparation method according to any one of claims 1 to 5 in the preparation of polymer flame retardant materials.

8. The use according to claim 7, characterized in that: The preparation method of the polymer flame retardant material is: The polymer material is first heated and melted, and then the nano-layered elemental phosphorus flame retardant is added, stirred evenly and pressed into shape; or the nano-layered elemental phosphorus flame retardant is first added before the monomer of the polymer material is polymerized, and then stirred evenly and polymerized into shape.

9. The use according to claim 8, characterized in that: The added amount of the nano-layered elemental phosphorus flame retardant accounts for 0.1% to 10% of the mass of the polymer material.

10. The use according to claim 8, characterized in that: The polymer material is selected from any one of epoxy resin, polyurethane and ethylene-vinyl acetate copolymer.

Citation Information

Patent Citations

  • Method used for low temperature batch synthesis of black phosphorus nanometer sheet material

    CN107188141A

  • Method for solvothermal preparation of two-dimensional black phosphorus nanometer material

    CN109850859A

  • Composite phosphorene flame retardant, flame retardant polymer composite material and preparation method thereof

    CN110194851A

  • Low-cost high-crystallinity black phosphorus and preparation method thereof

    CN111483990A

  • Nanometer layered simple-substance phosphorus flame retardant for macromolecular flame-retardant material as well as preparation method and application of nanometer layered simple-substance phosphorus flame retardant

    CN116376109A