Metal material and manufacturing method therefor, and television appearance structural member and manufacturing method therefor
By forming a first magnetron sputtering layer of nickel or titanium and a second magnetron sputtering layer of carbides on a metal substrate, and covering it with a resin layer, the problem of scratches on the exterior structural parts of TVs during sheet metal processing is solved, improving scratch resistance and aesthetics.
Patent Information
- Application Number
- PCT/CN2024/078498
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-02-26
- Publication Date
- 2024-11-14
AI Technical Summary
TV exterior structural components are prone to scratches during sheet metal processing, affecting their appearance.
A first magnetron sputtering layer with nickel or titanium plated on the surface of a metal substrate is used, a second magnetron sputtering layer of carbide, nitride or metal oxide is disposed opposite to it, and a resin layer is covered on it, forming a strong bond through magnetron sputtering.
It improves the hardness and scratch resistance of metal materials, prevents the sputtered layer from oxidizing and peeling off during sheet metal processing, and enhances the aesthetics and durability of the TV's exterior structural components.
Smart Images

Figure CN2024078498_14112024_PF_FP_ABST
Abstract
Description
Metal material and preparation method thereof, television appearance structural part and preparation method thereof
[0001] This application claims priority to the Chinese patent application filed with the China Patent Office on May 10, 2023, with application number 202310525405.6 and invention name “Metal material and preparation method thereof, television appearance structural part and preparation method thereof”, the entire contents of which are incorporated herein by reference. Technical Field
[0002] The present application relates to the field of home appliances, and in particular to a metal material and a preparation method thereof, a television appearance structural part and a preparation method thereof. Background Art
[0003] Television is one of the commonly used home appliances in people's lives. When people choose and buy a television, the appearance of the television is one of the important factors they consider. Technical issues
[0004] In the prior art, TV exterior components such as bases, back panels, and frames are typically made of pre-coated metal (PCM) sheets. However, these components typically require sheet metal processing such as stamping, stretching, and bending to form them. PCM sheets are prone to scratches during this process, which can negatively impact the TV's appearance.
[0005] Therefore, the existing technology needs to be improved and enhanced. Technical Solutions
[0006] The embodiments of the present application provide a metal material and a preparation method thereof, a television appearance structural component and a preparation method thereof, which can improve the scratch resistance of the television appearance structural component.
[0007] In a first aspect, an embodiment of the present application provides a metal material, including:
[0008] Metal substrate;
[0009] A first magnetron sputtering layer is provided on the surface of the metal substrate, wherein the first magnetron sputtering layer comprises at least one of nickel and titanium;
[0010] a second magnetron sputtering layer, disposed on a surface of the first magnetron sputtering layer facing away from the metal substrate, the second magnetron sputtering layer comprising at least one of carbide, nitride, pure metal and metal oxide; and
[0011] The resin layer is arranged on a surface of the second magnetron sputtering layer that is opposite to the first magnetron sputtering layer.
[0012] In a second aspect, an embodiment of the present application further provides a method for preparing a metal material, which is used to prepare any of the above-mentioned metal materials, comprising the following steps:
[0013] Providing a metal substrate;
[0014] forming a first magnetron sputtering layer on the surface of the metal substrate by magnetron sputtering, wherein the first magnetron sputtering layer comprises at least one of nickel and titanium;
[0015] forming a second magnetron sputtering layer on a surface of the first magnetron sputtering layer facing away from the metal substrate by magnetron sputtering, wherein the second magnetron sputtering layer comprises at least one of carbide, pure metal and metal oxide;
[0016] A resin layer is formed on a surface of the second magnetron sputtering layer that is opposite to the first magnetron sputtering layer.
[0017] In a third aspect, an embodiment of the present application further provides a television appearance structural part, wherein the television appearance structural part is made of a metal material manufactured by any of the above-mentioned methods for preparing a metal material, and the resin layer is located on the outer surface of the television appearance structural part.
[0018] In a fourth aspect, an embodiment of the present application further provides a method for preparing a television exterior structural component, comprising the following steps:
[0019] Providing a metal material manufactured by the method for preparing the metal material as described in any one of the above;
[0020] The metal material is made into the television appearance structural component through a sheet metal process. Beneficial effects
[0021] In an embodiment of the present application, the second magnetron sputtering layer with higher hardness is firmly bonded to the metal substrate through the first magnetron sputtering layer, thereby increasing the hardness of the metal material and further improving the scratch resistance of the metal material; further, due to the high bonding force between the resin layer and the second magnetron sputtering layer, the resin layer can be firmly bonded to the second magnetron sputtering layer during the sheet metal processing of the television exterior structural parts, thereby providing protection for the second magnetron sputtering layer, thereby preventing the second magnetron sputtering layer from being damaged by oxidation, and ultimately further improving the scratch resistance of the metal material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] FIG1 is a schematic diagram of the structure of the metal material provided in an embodiment of the present application.
[0023] FIG2 is a flow chart of a method for preparing a metal material provided in an embodiment of the present application.
[0024] FIG3 is a schematic diagram of the process of preparing the metal material shown in FIG2 .
[0025] FIG4 is a flow chart of a method for preparing a television exterior structural component provided in an embodiment of the present application.
[0026] The numbers in the figure are:
[0027] 100. Metal materials;
[0028] 11. Metal substrate; 12. First magnetron sputtering layer; 13. Second magnetron sputtering layer; 14. Resin layer;
[0029] 200, cleaning tank;
[0030] 21. Degreasing tank; 22. Water washing tank;
[0031] 300, baking area;
[0032] 400. Vacuum chamber equipment;
[0033] 41. First vacuum chamber; 42. Second vacuum chamber; 43. Third vacuum chamber;
[0034] 500. Roller coating area. Modes for Carrying Out the Invention
[0035] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the embodiments described are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative efforts are within the scope of protection of this application.
[0036] Please refer to Figure 1, which is a schematic diagram of the structure of a metal material provided in an embodiment of the present application. This embodiment of the present application provides a metal material 100 to improve the scratch resistance of the metal material 100. For example, the metal material 100 can be used in sheet metal parts. Therefore, when the metal material 100 is subjected to sheet metal processing operations such as stamping, stretching, and bending, the stamping die, stretching die, and bending die are prevented from scratching the sheet metal part.
[0037] The metal material 100 may include a metal substrate 11, a first magnetron sputtering layer 12, a second magnetron sputtering layer 13, and a resin layer 14. The first magnetron sputtering layer 12 is disposed on the surface of the metal substrate 11 and comprises at least one of nickel and titanium. The second magnetron sputtering layer 13 is disposed on the side of the first magnetron sputtering layer 12 facing away from the metal substrate 11 and comprises at least one of carbide, nitride, pure metal, and metal oxide. The resin layer 14 is disposed on the side of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12.
[0038] First, since the first magnetron sputtering layer 12 is a coating formed by magnetron sputtering, the first magnetron sputtering layer 12 is stacked at the atomic level, and there is still a certain free volume between the atoms of the first magnetron sputtering layer 12, so that the first magnetron sputtering layer 12 can improve the bonding force between the metal substrate 11 and the second magnetron sputtering layer 13, and since the first magnetron sputtering layer 12 is a metal titanium (Ti) and / or nickel (Ni) with high ductility, the first magnetron sputtering layer 12 is not easy to fall off or break during the bending process of the TV appearance structural parts, thereby further improving the bonding force between the metal substrate 11 and the second magnetron sputtering layer 13.
[0039] Since the second magnetron sputtered layer 13 includes at least one of carbide, pure metal, and metal oxide, it has a relatively high hardness, thereby significantly increasing the overall hardness of the metal material 100 and thereby improving the scratch resistance of the metal material 100. Furthermore, since carbide, pure metal, and metal oxide have excellent ductility, the second magnetron sputtered layer 13 is less likely to fall off or crack during the bending of the television exterior structural component, thereby further improving the bonding strength and stability between the first magnetron sputtered layer 12 and the second magnetron sputtered layer 13.
[0040] Next, since the second magnetron sputtering layer 13 is a coating formed by magnetron sputtering, the second magnetron sputtering layer 13 is stacked at the atomic level, and there is still a certain free volume between the atoms of the second magnetron sputtering layer 13, so that the second magnetron sputtering layer 13 can improve the bonding force between the first magnetron sputtering layer 12 and the resin layer, and since the second magnetron sputtering layer 13 includes at least one of carbides, pure metals and metal oxides with high ductility, the second magnetron sputtering layer 13 is not easy to fall off or break during the bending process of the TV appearance structure.
[0041] Finally, the resin layer 14 can prevent the second magnetron sputtering layer 13 from being damaged by oxidation, corrosion, etc.
[0042] To sum up, the embodiment of the present application can firmly bond the second magnetron sputtering layer 13 with higher hardness to the metal substrate 11 through the first magnetron sputtering layer 12, thereby improving the hardness of the metal material 100, and then improving the scratch resistance of the metal material 100. The resin layer 14 can prevent the second magnetron sputtering layer 13 from being damaged by oxidation, corrosion, etc., and ultimately further improve the scratch resistance of the metal material.
[0043] In some embodiments, the metal substrate 11 may be made of metal materials such as steel, aluminum, aluminum alloy, etc., which is not limited in the embodiments of the present application.
[0044] In some embodiments, in order to improve the bonding strength between the metal substrate 11 and the first magnetron sputtering layer 12 , the metal substrate 11 may not have an oxide film layer, so that the first magnetron sputtering layer 12 is closely attached to the body of the metal substrate 11 .
[0045] In some embodiments, the thickness of the first magnetron sputtering layer 12 is greater than or equal to 0.8 μm and less than or equal to 1.2 μm. It is understood that, on the one hand, by controlling the thickness of the first magnetron sputtering layer 12, the manufacturing cost of the first magnetron sputtering layer 12 can be reduced; on the other hand, by controlling the thickness of the first magnetron sputtering layer 12, it is possible to avoid the first magnetron sputtering layer 12 being too thin, which would result in excessive internal stress in the first magnetron sputtering layer 12, thereby reducing the adhesion between the metal substrate 11 and the second magnetron sputtering layer 13, and to avoid the first magnetron sputtering layer 12 being too thin, which would result in cracking in the first magnetron sputtering layer 12 during the stamping or bending of the metal material 100.
[0046] For example, the thickness of the first magnetron sputtering layer 12 may be 0.8 μm, 0.84 μm, 0.89 μm, 0.91 μm, 0.92 μm, 0.94 μm, 0.96 μm, 0.99 μm, 1.08 μm, 1.11 μm, 1.18 μm or 1.2 μm, which is not limited in the embodiments of the present application.
[0047] It can also be understood that the above-mentioned first magnetron sputtering layer 12 includes at least one of nickel and titanium materials. It can be: the first magnetron sputtering layer 12 includes nickel material and does not include titanium material, or the first magnetron sputtering layer 12 includes titanium material and does not include nickel material, or some areas of the first magnetron sputtering layer 12 are nickel material and some areas are titanium material. The embodiment of the present application does not limit this.
[0048] Specifically, the first magnetron sputtering layer 12 may be solely composed of nickel or titanium, so as to meet the bonding force and ductility requirements of the first magnetron sputtering layer 12 , which is not limited in the embodiment of the present application.
[0049] In some embodiments, the thickness of the second magnetron sputtering layer 13 may be greater than or equal to 30 nm and less than or equal to 500 nm.
[0050] It is understood that, on the one hand, the thickness of the second magnetron sputtering layer 13 is between 30 nm and 500 nm, which can well ensure the hardness of the second magnetron sputtering layer 13, thereby providing the metal material 100 with sufficient scratch resistance. On the other hand, by adjusting the thickness of the second magnetron sputtering layer 13, the color of the second magnetron sputtering layer 13 can be adjusted. For example, taking the second magnetron sputtering layer 13 as an example, by gradually increasing the thickness of the second magnetron sputtering layer 13, the overall color of the metal material 100 can be gradually changed from light yellow to dark yellow, and finally to black.
[0051] For example, the thickness of the second magnetron sputtering layer 13 can be 30nm, 45.6nm, 58nm, 79.5nm, 92.3nm, 114.5nm, 130nm, 148nm, 176nm, 199nm, 223nm, 248nm, 286nm, 304nm, 310nm, 324nm, 343nm, 374nm, 392nm, 400nm, 411nm, 432nm, 451nm, 477.8nm or 500nm, which is not limited to the embodiments of the present application.
[0052] In some embodiments, the thickness of the second magnetron sputtering layer 13 is greater than or equal to 80 nm and less than or equal to 120 nm. This allows the second magnetron sputtering layer 13 to form an island chain structure, or in other words, allows the surface of the second magnetron sputtering layer 13 to have a certain concave-convex structure and cavities, so that the resin layer 14 can be more firmly anchored to the second magnetron sputtering layer 13 and is not easily detached during sheet metal processing.
[0053] For example, the thickness of the second magnetron sputtering layer 13 may be 80 nm, 84.6 nm, 87.7 nm, 89.2 nm, 92.3 nm, 94.4 nm, 100.6 nm, 103.7 nm, 109 nm, 114.5 nm or 120 nm, etc., which is not limited in the embodiments of the present application.
[0054] In some embodiments, the second magnetron sputtering layer 13 is made of at least one of titanium nitride (TiN), titanium carbonitride (TiCN), chromium carbide (Cr3C2), nickel (Ni), titanium (Ti), and titanium dioxide (TiO2).
[0055] It can be understood that titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium and titanium dioxide materials not only have the advantages of high brightness and strong metallic luster, but also have the advantage of high ductility, so that the second magnetron sputtering layer 13 can be more firmly arranged on the first magnetron sputtering layer 12, and is not easy to break or fall off during sheet metal processing.
[0056] It can also be understood that the second magnetron sputtering layer 13 is at least one of titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium and titanium dioxide materials, and it can be that the second magnetron sputtering layer 13 is only formed of one of titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium and titanium dioxide materials.
[0057] For example, the second magnetron sputtering layer 13 may consist only of titanium nitride.
[0058] Optionally, the second magnetron sputtering layer 13 is at least one of titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium and titanium dioxide materials. It can also be that different parts of the second magnetron sputtering layer 13 are composed of different materials among titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium and titanium dioxide materials. This embodiment of the present application is not limited to this.
[0059] In some embodiments, the elongation of the resin layer 14 can be greater than or equal to 100%, so that the resin layer 14 has good ductility, thereby preventing the metal material 100 from breaking or falling off from the second magnetron sputtering layer 13 during sheet metal processing steps such as bending, stretching, and stamping.
[0060] Exemplarily, the elongation of the resin layer 14 can be 100%, 103%, 107%, 109.1%, 110%, 113%, 117.8%, 119.2%, 133%, 136%, 142%, 146%, 151.2%, 159%, 160%, 166.5%, 169.7%, 170%, 175%, 180% or 181%, etc., which is not limited to the embodiments of the present application.
[0061] Of course, in actual use, the elongation of the resin layer 14 may be greater than or equal to 110%, or the elongation of the resin layer 14 may be greater than or equal to 120%, and this embodiment of the present application does not limit this.
[0062] In some embodiments, the elongation of the resin layer 14 may be less than or equal to 150%, for example, the elongation of the resin layer 14 may be 133%, 136%, 142%, 146%, or 150%, etc., which is not limited in the present embodiment.
[0063] As can be understood, taking the example of metal material 100 used in a television exterior structural component, when sheet metal processing is performed on the metal material 100, an elongation of the resin layer 14 between 100% and 150% can meet the actual processing requirements of television exterior structural components. This makes the resin layer 14 less likely to crack or fall off during sheet metal processing steps such as bending, stretching, and stamping. Furthermore, an elongation of the resin layer 14 of less than or equal to 150% can also reduce the cost of the resin layer 14.
[0064] In some embodiments, the resin layer 14 may be made of silicone-modified polyurethane.
[0065] It can be understood that, on the one hand, the organosilicon-modified polyurethane has the advantages of high adhesion and high ductility, so that the resin layer 14 can be more firmly arranged on the second magnetron sputtering layer 13, and is not easy to crack or fall off during sheet metal processing. On the second hand, the organosilicon-modified polyurethane has the advantages of good mechanical properties and high gloss, so it can further improve the scratch resistance of the metal material 100 and improve the aesthetics of the metal material 100. On the third hand, the organosilicon-modified polyurethane has the advantages of wear resistance, oil resistance, cold resistance, tear resistance, chemical corrosion resistance, high temperature resistance, organic solvent resistance and fingerprint resistance, which can well ensure that the metal material 100 is not easily contaminated during subsequent use.
[0066] In some embodiments, when the resin layer 14 includes silicone-modified polyurethane, the molecular weight of the silicone-modified polyurethane can be greater than or equal to 5,000 and less than or equal to 20,000, so as to further improve the ductility of the resin layer 14, so that the resin layer 14 can be more firmly arranged on the second magnetron sputtering layer 13, and is not easy to break or fall off during sheet metal processing.
[0067] For example, the molecular weight of the silicone-modified polyurethane can be 5000, 5320, 5886, 6110, 6223, 6664, 7145, 7632, 8190, 8345, 9100, 9200, 9425, 9746, 9883, 9945, 10000, 10050, 11000, 11321, 12410, 13320, 14520, 15320, 15886, 16210, 16265, 17245, 17632, 18220, 18375, 19102, 19208, 19435, 19889 or 20000, which is not limited in the embodiments of the present application.
[0068] In some embodiments, when the resin layer 14 includes silicone-modified polyurethane, the silicone-modified polyurethane can be a dendritic polymer. Of course, it can also be understood that the silicone-modified polyurethane is a dendritic polymer or a hyperbranched polymer. It is understandable that the dendritic polymer has good fluid properties and is easy to process, and can be more evenly coated on the second magnetron sputtering layer 13, so that the surface of the second magnetron sputtering layer 13 is formed with a resin layer 14 with a more uniform thickness in various places, so as to prevent the thickness of some areas of the resin layer 14 from being insufficient, thereby causing the area to break when sheet metal processing is performed. At the same time, the dendritic polymer can further improve the ductility of the resin layer 14, so that the resin layer 14 can be more firmly arranged on the second magnetron sputtering layer 13, and is not easy to break or fall off when sheet metal processing is performed.
[0069] Of course, in some other embodiments, the resin layer 14 may also be made of other acrylic resins, other types of modified polyurethane resins, etc., which is not limited in the embodiments of the present application.
[0070] In some embodiments, the resin layer 14 may be transparent, so that the brightness and gloss of the second magnetron sputtering layer 13 can be better displayed, thereby improving the aesthetics of the metal material 100 .
[0071] In some embodiments, the resin layer 14 may be transparent and may be added with a colorant, thereby adjusting the color exhibited by the metal material 100 through the colorant.
[0072] For example, after the toner is added to the resin layer 14 , the resin layer 14 may exhibit the same color as the second magnetron sputtered layer 13 , thereby deepening the color exhibited by the second magnetron sputtered layer 13 .
[0073] Alternatively, the resin layer 14 may exhibit a color different from that of the second magnetron sputtering layer 13 after adding a colorant, thereby mixing with the second magnetron sputtering layer 13 to form a different color, which is not limited in the embodiment of the present application.
[0074] In some embodiments, the thickness of the resin layer 14 may be greater than or equal to 10 μm, so that the resin layer 14 has sufficient thickness to provide sufficient protection for the second magnetron sputtering layer 13 .
[0075] For example, the thickness of the resin layer 14 can be 10μm, 11.2μm, 11.7μm, 12.1μm, 13.3μm, 13.8μm, 14μm, 16μm, 17μm, 18μm, 18.7μm, 19.2μm, 19.8μm, 20μm, 24μm, 28μm, 30μm, 40μm, etc., which is not limited to the embodiments of the present application.
[0076] In some embodiments, the thickness of the resin layer 14 can be less than or equal to 20 μm. This can prevent the increased difficulty and high cost of manufacturing the resin layer 14 due to an excessive thickness. Furthermore, when the resin layer 14 is made of a light-transmitting material, this can also prevent the decreased transparency of the resin layer 14 due to an excessive thickness. This allows the gloss and brightness of the second magnetron sputtered layer 13 to be well displayed, thereby enhancing the aesthetics of the metal material 100.
[0077] For example, the thickness of the resin layer 14 may be 10 μm, 11.2 μm, 11.7 μm, 12.1 μm, 13.3 μm, 13.8 μm, 14 μm, 16 μm, 17 μm, 18 μm, 18.7 μm, 19.2 μm, 19.8 μm or 20 μm, which is not limited in the embodiments of the present application.
[0078] In some embodiments, the first magnetron sputtering layer 12 is made of nickel or titanium, and the thickness of the first magnetron sputtering layer 12 is greater than or equal to 0.8 μm and less than or equal to 1.2 μm. The second magnetron sputtering layer 13 is made of titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium, or titanium dioxide, and the thickness of the second magnetron sputtering layer 13 is greater than or equal to 30 nm and less than or equal to 500 nm. The elongation of the resin layer 14 is between 100% and 150%, and the thickness of the resin layer 14 is greater than or equal to 10 μm and less than or equal to 20 μm. The resin layer 14 includes a silicone-modified polyurethane material, and the molecular weight of the silicone-modified polyurethane is greater than or equal to 5000 and less than or equal to 20000. The silicone-modified polyurethane is a dendrimer. Then, the performance parameters of the metal material 100 can be as shown in the following table:
[0079] Table 1. Performance parameters of metal material 100
[0080] Please continue to refer to Figure 2, which is a flow chart of a method for preparing a metal material provided in an embodiment of the present application. The embodiment of the present application also provides a method for preparing a metal material, which is used to prepare the above-mentioned metal material 100, comprising the following steps:
[0081] S101 , providing a metal substrate 11 .
[0082] Please continue to refer to Figure 3, which is a schematic diagram of the process of preparing the metal material shown in Figure 2. In some embodiments, providing the metal substrate 11 may include: providing a metal substrate coil; and uncoiling the metal substrate coil.
[0083] For example, the metal substrate coil can be a steel coil with a thickness of 0.4 mm, a width of 1280 mm, and a grade of 201J1. During use, the free end of the steel coil can be welded to the traction belt of the traction device, and then the traction device can be activated to traction and unwind.
[0084] Alternatively, providing the metal substrate 11 may further include providing a metal substrate plate.
[0085] It is understandable that the embodiment of the present application does not limit the shape of the metal substrate 11.
[0086] S102 , forming a first magnetron sputtering layer 12 on the surface of the metal substrate 11 by magnetron sputtering, wherein the first magnetron sputtering layer 12 includes at least one of nickel and titanium.
[0087] In some embodiments, forming the first magnetron sputtering layer 12 on the surface of the metal substrate 11 by magnetron sputtering may further include: placing the metal substrate 11 into a cleaning tank 200 for cleaning. This cleans the oxide film, stains, etc. on the surface of the metal substrate 11 and makes the surface of the metal substrate 11 smoother, thereby improving the bonding strength between the first magnetron sputtering layer 12 and the metal substrate 11.
[0088] In some embodiments, the metal substrate 11 is sent into the cleaning tank 200 for cleaning, which may include: cleaning the metal substrate 11 with a degreasing solution; and washing the metal substrate 11 cleaned with the degreasing solution with water.
[0089] For example, the cleaning tank 200 may include a degreasing tank 21 and a water washing tank 22. The metal substrate 11 is sequentially placed in the degreasing tank 21 and the water washing tank 22 for cleaning. The cleaning liquid in the degreasing tank 21 may be a degreasing liquid having a pH value greater than or equal to 8 and less than or equal to 12, and a temperature greater than or equal to 30°C and less than or equal to 50°C. The cleaning liquid in the water washing tank 22 may be water to clean any residual degreasing liquid from the surface of the metal substrate 11.
[0090] In some embodiments, the metal substrate 11 is sent into the cleaning tank 200 for cleaning, which may include: cleaning the metal substrate 11 by at least one of plasma cleaning and ultrasonic vibration cleaning to improve the cleaning effect.
[0091] Specifically, plasma cleaning and / or ultrasonic oscillation cleaning can be performed in the degreasing tank 21, or plasma cleaning and / or ultrasonic oscillation cleaning can be performed in the water washing tank 22, or plasma cleaning and / or ultrasonic oscillation cleaning can be performed in both the degreasing tank 21 and the water washing tank 22 at the same time. This embodiment of the present application does not limit this.
[0092] In some embodiments, after the metal substrate 11 is sent to the cleaning tank 200 for cleaning, the process may further include sending the metal substrate 11 to the baking area 300 for drying, thereby increasing the drying speed of the metal substrate 11 .
[0093] Illustratively, the drying temperature of the baking zone 300 may be greater than or equal to 100° C. and less than or equal to 140° C. For example, the drying temperature may be 100° C., 107° C., 109° C., 114° C., 116° C., 120° C., 125° C., 137° C., or 140° C., which is not limited in this embodiment of the present application.
[0094] In some embodiments, forming a first magnetron sputtering layer 12 on the surface of a metal substrate 11 by magnetron sputtering may include: providing a vacuum chamber device 400, the vacuum chamber device 400 including a plurality of first vacuum chambers 41, the plurality of first vacuum chambers 41 being connected in sequence so that the plurality of first vacuum chambers 41 form a channel for the metal substrate 11 to move along a first path, the first path including a first end and a second end relative to each other; along the first path, of any two adjacent first vacuum chambers 41, the vacuum degree of the first vacuum chamber 41 close to the first end is less than the vacuum degree of the first vacuum chamber 41 away from the first end; conveying the metal substrate 11 from the first end to the second end along the first path; and forming the first magnetron sputtering layer 12 by magnetron sputtering in the first vacuum chamber 41 located at the second end.
[0095] It is understandable that the first path can be a straight path or a curved path, and the embodiment of the present application does not limit this.
[0096] For example, the first path can be from left to right, or the metal substrate 11 can be fed into the vacuum chamber apparatus 400 from left to right. Then, the multiple first vacuum chambers 41 can be arranged from left to right. In other words, the metal substrate 11 is fed into the leftmost first vacuum chamber 41, passes through all the first vacuum chambers 41 in sequence, and then enters the rightmost first vacuum chamber 41, where magnetron sputtering is performed.
[0097] It is understood that, compared to the first vacuum chamber 41 at the far right, which is directly connected to the external environment, the embodiment of the present application, through the use of multiple first vacuum chambers 41 with gradually increasing vacuum levels, can significantly improve the leakage at the inlet of the first vacuum chamber 41 at the far right, thereby ensuring the purity and structural reliability of the generated first magnetron sputtering layer 12, and further improving the bonding strength between the metal substrate 11 and the second magnetron sputtering layer 13. Of course, the first vacuum chamber 41 at the far right can also be quickly evacuated to form a suitable vacuum level.
[0098] Specifically, the number of the multiple first vacuum chambers 41 may be three, four, five or even six, which is not limited in the embodiment of the present application.
[0099] In some embodiments, the vacuum degree of the first vacuum chamber 41 at the second end is greater than or equal to 1*10 -3 Pa and less than or equal to 1*10 -1 Pa. This ensures the purity and structural reliability of the generated first magnetron sputtering layer 12, thereby improving the bonding force between the metal substrate 11 and the second magnetron sputtering layer 13.
[0100] For example, the vacuum degree of the first vacuum chamber 41 may be 1*10 -3 Pa, 1*10 -2 Pa or 1*10 -1 Pa, this embodiment of the present application does not limit this.
[0101] Alternatively, the vacuum chamber equipment 400 may also have only one first vacuum chamber 41 instead of the above-mentioned multiple first vacuum chambers 41, so that the metal substrate 11 can be magnetron sputtered in the first vacuum chamber 41 to form a first magnetron sputtering layer 12. This embodiment of the present application is not limited to this.
[0102] S103 , forming a second magnetron sputtering layer 13 on a surface of the first magnetron sputtering layer 12 facing away from the metal substrate 11 by magnetron sputtering, wherein the second magnetron sputtering layer 13 includes at least one of carbide, pure metal, and metal oxide.
[0103] In some embodiments, the vacuum chamber apparatus 400 described above includes a first vacuum chamber 41 and may include multiple second vacuum chambers 42. The multiple second vacuum chambers 42 are sequentially connected to form a channel for the metal substrate 11 to move along a second path. The second path includes a third end and a fourth end. Along the second path, of any two adjacent second vacuum chambers 42, the vacuum level of the second vacuum chamber 42 closer to the third end is greater than the vacuum level of the second vacuum chamber 42 farther from the third end. Forming the resin layer 14 on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 further includes: forming the second magnetron sputtering layer 13 by magnetron sputtering in the second vacuum chamber 42 located at the third end; and transporting the metal substrate 11 formed with the second magnetron sputtering layer 13 along the second path.
[0104] It is understandable that the second path can be a straight path or a curved path, and the embodiment of the present application does not limit this.
[0105] For example, the second path may be from left to right, and the metal substrate 11 may be magnetron sputtered in the leftmost second vacuum chamber 42 and then sent out from the rightmost second vacuum chamber 42 along the second path.
[0106] It is understood that, compared to the leftmost second vacuum chamber 42 being directly connected to the external environment, the embodiment of the present application, through the use of multiple second vacuum chambers 42 with gradually increasing vacuum levels, can greatly reduce gas leakage at the outlet of the leftmost second vacuum chamber 42, thereby ensuring the purity and structural reliability of the generated second magnetron sputtering layer 13, thereby improving the scratch resistance of the metal material 100 and enhancing the bonding strength between the second magnetron sputtering layer 13 and the resin layer 14. Of course, the leftmost second vacuum chamber 42 can also be quickly evacuated to form a suitable vacuum level.
[0107] Specifically, the plurality of second vacuum chambers 42 may be three, four, five or even six, which is not limited in this embodiment of the present application.
[0108] The first vacuum chamber 41 at the second end and the second vacuum chamber 42 at the third end may be connected or separated, which is not limited in this embodiment of the present application.
[0109] Taking the example of a vacuum chamber apparatus 400 in which the first vacuum chamber 41 at the second end and the second vacuum chamber 42 at the third end are connected, the vacuum chamber apparatus 400 may further include a third vacuum chamber 43, which is connected to the first vacuum chamber 41 at the second end and the second vacuum chamber 42 at the third end, respectively. Before forming the second magnetron sputtering layer 13 by magnetron sputtering in the second vacuum chamber 42 at the third end, the preparation method further includes transferring the metal substrate 11 from the first vacuum chamber 41 at the second end to the second vacuum chamber 42 at the third end via the third vacuum chamber 43.
[0110] Thus, by connecting the first vacuum chamber 41 at the second end with the second vacuum chamber 42 at the third end via the third vacuum chamber 43, both the outlet of the first vacuum chamber 41 at the second end and the inlet of the second vacuum chamber 42 at the third end can be well sealed, thereby preventing the seals at the outlet of the first vacuum chamber 41 at the second end and the inlet of the second vacuum chamber 42 at the third end. This ensures the purity and structural reliability of the generated first magnetron sputtering layer 12 and the second magnetron sputtering layer 13, ultimately improving the scratch resistance of the metal material 100 and enhancing the bonding strength between the various layered structures.
[0111] Alternatively, the vacuum chamber equipment 400 may also include only the second vacuum chamber 42 without the first vacuum chamber 41 and the third vacuum chamber 43 .
[0112] Then, forming the resin layer 14 on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 can include: providing a vacuum chamber device 400, the vacuum chamber device 400 includes a plurality of second vacuum chambers 42, the plurality of second vacuum chambers 42 are connected in sequence so that the plurality of second vacuum chambers 42 form a channel for the metal substrate 11 to move along a second path, the second path includes a third end and a fourth end relative to each other; along the second path, of any two adjacent second vacuum chambers 42, the vacuum degree of the second vacuum chamber 42 close to the third end is greater than the vacuum degree of the second vacuum chamber 42 away from the third end; transporting the metal substrate 11 formed with the second magnetron sputtering layer 13 along the second path; and forming the second magnetron sputtering layer 13 by magnetron sputtering in the second vacuum chamber 42 located at the third end.
[0113] In some embodiments, the second vacuum chamber 42 at the third end is filled with an inert gas having a purity greater than or equal to 99.99%. The inert gas may include nitrogen. This ensures the purity and material properties of the second magnetron sputtered layer 13, thereby improving the scratch resistance of the metal material 100 and enhancing the bonding strength between the various layered structures.
[0114] For example, the inert gas filled in the second vacuum chamber 42 may include only nitrogen, and the second magnetron sputtering layer 13 may be formed of titanium nitride or other metal nitrides.
[0115] Alternatively, the inert gas may be a mixture of nitrogen and argon, which is not limited in the embodiments of the present application.
[0116] It can also be understood that, in combination with the above-mentioned vacuum chamber equipment 400, which may include a first vacuum chamber 41 and a third vacuum chamber 43, since the first vacuum chamber 41 does not need to be filled with nitrogen, the third vacuum chamber 43 can well separate the first vacuum chamber 41 at the second end from the second vacuum chamber 42 at the third end, so as to prevent nitrogen from directly entering the first vacuum chamber 41 at the second end, thereby avoiding the nitrogen in the second vacuum chamber 42 from interfering with the first magnetron sputtering layer 12 formed in the first vacuum chamber 41.
[0117] The vacuum degree of the third vacuum chamber 43 may be greater than that of the first vacuum chamber 41 at the second end.
[0118] S104 , forming a resin layer 14 on a surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 .
[0119] In some embodiments, forming the resin layer 14 on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 may include: coating the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 with silicone-modified polyurethane, so that the silicone-modified polyurethane forms the resin layer 14 after drying.
[0120] The organosilicon-modified polyurethane may be applied by roller coating in the roller coating area 500 to make the thickness of the resin layer 14 more uniform. Of course, the organosilicon-modified polyurethane may also be applied by spraying, which is not limited in the present embodiment.
[0121] In some embodiments, after forming the resin layer 14 on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12, the method may further include curing the silicone-modified polyurethane on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 by a UV curing process.
[0122] Alternatively, the organosilicon-modified polyurethane on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 may also be naturally cured, which is not limited in the embodiment of the present application.
[0123] In some embodiments, taking the metal substrate 11 as a coil, after forming the resin layer 14 on the surface of the second magnetron sputtering layer 13 facing away from the first magnetron sputtering layer 12 , the method may further include: rolling up the metal substrate 11 for easy turnover.
[0124] The embodiment of the present application further provides a television appearance structural component, which is made of the metal material 100 manufactured by the above-mentioned metal material preparation method, and the resin layer 14 is located on the outer surface of the television appearance structural component.
[0125] The outer surface of the television exterior structural component may include a curved surface, and the bending radius of the curved surface may be less than 1.5 mm, thereby ensuring that the outer surface of the metal material 100 will not be scratched, cracked, or have the film layer fall off.
[0126] Among them, the TV appearance structural parts may include the TV base cover, TV back panel, TV middle frame, TV front frame or TV rear shell, etc., which is not limited in the embodiments of the present application.
[0127] Please continue to refer to Figure 4, which is a flow chart of a method for preparing a television exterior structural component provided by an embodiment of the present application. The present application also provides a method for preparing a television exterior structural component, comprising the following steps:
[0128] S201. Provide a metal material 100 manufactured by the above-mentioned method for preparing the metal material.
[0129] S202 , manufacturing the metal material 100 into a television exterior structural component through a sheet metal process.
[0130] The resin layer 14 is located on the outer surface of the television exterior structural component.
[0131] In some embodiments, the sheet metal process may include at least one of stamping, blanking, curling, flanging, stretching, and bending, which is not limited in the embodiments of the present application.
[0132] In some embodiments, making the metal material 100 into a television appearance structural component through a sheet metal process may include: processing the metal material 100 through a sheet metal process to form a first intermediate; and laminating an inner lining to the surface of the metal substrate 11 of the first intermediate facing away from the first magnetron sputtering layer 12.
[0133] For example, the lining may include galvanized sheet, insulating sheet, buffer sheet, etc., which is not limited in the embodiment of the present application.
[0134] In the above embodiments, the description of each embodiment has its own focus. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0135] The above is a detailed introduction to the metal materials and their preparation methods, television appearance structural parts and their preparation methods provided in the embodiments of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technical personnel in this field, based on the ideas of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A metal material comprising: Metal substrate; A first magnetron sputtering layer is disposed on the surface of the metal substrate, wherein the first magnetron sputtering layer comprises at least one of nickel and titanium; A second magnetron sputtering layer is disposed on a surface of the first magnetron sputtering layer that is opposite to the metal substrate, wherein the second magnetron sputtering layer comprises at least one of carbide, nitride, pure metal and metal oxide; and The resin layer is disposed on a surface of the second magnetron sputtering layer that is opposite to the first magnetron sputtering layer.
2. The metal material according to claim 1, wherein: The elongation of the resin layer is greater than or equal to 100% and less than or equal to 150%.
3. The metal material according to claim 2, wherein: The resin layer includes an organosilicon-modified polyurethane material, the molecular weight of the organosilicon-modified polyurethane is greater than or equal to 5000 and less than or equal to 20000, and the organosilicon-modified polyurethane is a dendritic polymer.
4. The metal material according to claim 1, wherein: The resin layer has a thickness greater than or equal to 10 μm and less than or equal to 20 μm.
5. The metal material according to claim 1, wherein The thickness of the first magnetron sputtering layer is greater than or equal to 0.8 μm and less than or equal to 1.2 μm.
6. The metal material according to claim 1, wherein The thickness of the second magnetron sputtering layer is greater than or equal to 30 nm and less than or equal to 500 nm.
7. The metal material according to claim 1, wherein: The second magnetron sputtering layer is made of at least one of titanium nitride, titanium carbonitride, chromium carbide, nickel, titanium and titanium dioxide.
8. A method for preparing a metal material, for preparing the metal material as claimed in claim 1, comprising the following steps: Providing a metal substrate; Forming a first magnetron sputtering layer on the surface of the metal substrate by magnetron sputtering, wherein the first magnetron sputtering layer includes at least one of nickel and titanium; Forming a second magnetron sputtering layer on a surface of the first magnetron sputtering layer facing away from the metal substrate by magnetron sputtering, wherein the second magnetron sputtering layer includes at least one of carbide, pure metal and metal oxide; A resin layer is formed on a surface of the second magnetron sputtering layer that is opposite to the first magnetron sputtering layer.
9. The method for preparing a metal material according to claim 8, wherein: The step of forming a first magnetron sputtering layer on the surface of the metal substrate by magnetron sputtering comprises: A vacuum chamber device is provided, the vacuum chamber device comprising a plurality of first vacuum chambers, the plurality of first vacuum chambers being connected in sequence so that a channel is formed in the plurality of first vacuum chambers for the metal substrate to move along a first path, the first path comprising a first end and a second end opposite to each other; along the first path, of any two adjacent first vacuum chambers, the vacuum degree of the first vacuum chamber close to the first end is less than the vacuum degree of the first vacuum chamber far from the first end; conveying the metal substrate along the first path from the first end to the second end; The first magnetron sputtering layer is formed by magnetron sputtering in a first vacuum chamber located at the second end.
10. The method for preparing a metal material according to claim 8, wherein: The vacuum degree of the first vacuum chamber located at the second end is greater than or equal to 1*10 -3 Pa and less than or equal to 1*10 -1 Pa.
11. The method for preparing a metal material according to claim 8, wherein: The vacuum chamber equipment further includes a plurality of second vacuum chambers, which are connected in sequence so that the plurality of second vacuum chambers form a channel for the metal substrate to move along a second path, wherein the second path includes a third end and a fourth end opposite to each other; along the second path, of any two adjacent second vacuum chambers, the vacuum degree of the second vacuum chamber close to the third end is greater than the vacuum degree of the second vacuum chamber far from the third end; The method of forming a resin layer on a surface of the second magnetron sputtering layer facing away from the first magnetron sputtering layer further comprises: forming the second magnetron sputtering layer by magnetron sputtering in a second vacuum chamber located at the third end; The metal substrate having the second magnetron sputtering layer formed thereon is transported along the second path.
12. The method for preparing a metal material according to claim 11, wherein: The vacuum chamber equipment further includes a third vacuum chamber, and the third vacuum chamber is respectively connected to the first vacuum chamber located at the second end and the second vacuum chamber located at the third end; Before forming the second magnetron sputtering layer by magnetron sputtering in the second vacuum chamber located at the third end, the preparation method further includes: transporting the metal substrate in the first vacuum chamber located at the second end to the second vacuum chamber located at the third end through the third vacuum chamber.
13. The method for preparing a metal material according to claim 8, wherein: The method of forming a resin layer on a surface of the second magnetron sputtering layer facing away from the first magnetron sputtering layer further comprises: A vacuum chamber device is provided, the vacuum chamber device comprising a plurality of second vacuum chambers, the plurality of second vacuum chambers are sequentially connected so that the plurality of second vacuum chambers form a channel for the metal substrate to move along a second path, the second path comprising a third end and a fourth end opposite to each other; along the second path, of any two adjacent second vacuum chambers, the vacuum degree of the second vacuum chamber close to the third end is greater than the vacuum degree of the second vacuum chamber far from the third end; conveying the metal substrate having the second magnetron sputtering layer formed thereon along the second path; The second magnetron sputtering layer is formed by magnetron sputtering in a second vacuum chamber located at the third end.
14. The method for preparing a metal material according to claim 11, wherein: The second vacuum chamber located at the third end is filled with an inert gas, the purity of the inert gas is greater than or equal to 99.99%, and the inert gas includes nitrogen.
15. The method for preparing a metal material according to claim 11, wherein: The forming of a resin layer on a surface of the second magnetron sputtering layer facing away from the first magnetron sputtering layer comprises: The organosilicon-modified polyurethane is coated on the surface of the second magnetron sputtering layer which is opposite to the first magnetron sputtering layer, so that the organosilicon-modified polyurethane forms the resin layer after being dried.
16. A television appearance structural component, wherein the television appearance structural component is made of a metal material manufactured by the method for preparing a metal material according to claim 8, wherein the resin layer is located on an outer surface of the television appearance structural component.
17. The television appearance structural member according to claim 16, wherein: The elongation of the resin layer is greater than or equal to 100% and less than or equal to 150%.
18. The television appearance structural member according to claim 16, wherein: The resin layer includes an organosilicon-modified polyurethane material, the molecular weight of the organosilicon-modified polyurethane is greater than or equal to 5000 and less than or equal to 20000, and the organosilicon-modified polyurethane is a dendritic polymer.
19. The television appearance structural member according to claim 16, wherein: The resin layer has a thickness greater than or equal to 10 μm and less than or equal to 20 μm.
20. A method for preparing a television appearance structural component, comprising the following steps: Providing a metal material manufactured by the preparation method according to claim 8; The metal material is made into the television appearance structural component through a sheet metal process.
Citation Information
Patent Citations
Vacuum coating part and preparation method thereof
CN102345102A
Metal foil continuous film-coating device
CN103074592A
Film-coating member and manufacturing method thereof
CN103184410A
Shell and manufacturing method thereof
CN103935075A
Metal material and preparation method thereof, and television appearance structural member and preparation method thereof
CN117403197A