[0037] Embodiment 1, fiber treatment modifier, prepared from the following raw materials, specifically:
[0038] N-methylolacrylamide 8% (owf);
[0040] The bath ratio is 1:10.
[0041] Wherein, the modifying agent for fiber treatment in this embodiment 1 can modify the fiber material according to the following modification method. Specifically, the fiber modification method includes the following process steps:
[0042] a. Put the modifier in clear water to obtain a modifier solution. The modifier is prepared from the following raw materials, specifically:
[0043] N-methylolacrylamide 8% (owf);
[0044] Zinc chloride 8g / L;
[0045] Bath ratio 1:10;
[0046] b. Soak the fiber material in the modifier solution for 30 minutes;
[0047] c. After the fiber material is soaked, dry the fiber material at a temperature of 90 degrees Celsius.
[0048] The modifier for fiber treatment and the modification method thereof in the first embodiment can effec...
Embodiment 2
[0049] Embodiment 2, the modifying agent for fiber treatment, is prepared from the following raw materials, specifically:
[0050] N-methylolacrylamide 13% (owf);
[0051] Zinc chloride 11;
[0052] The bath ratio is 1:15.
[0053] Wherein, the modifying agent for fiber treatment in this embodiment 2 can modify the fiber material according to the following modification method. Specifically, the fiber modification method includes the following process steps:
[0054] a. Put the modifier in clear water to obtain a modifier solution. The modifier is prepared from the following raw materials, specifically:
[0055] N-methylolacrylamide 13% (owf);
[0056] Zinc chloride 11g / L;
[0057] Bath ratio 1:15;
[0058] b. Soak the fiber material in the modifier solution for 15 minutes;
[0059] c. After the fiber material is soaked, dry the fiber material at a temperature of 90 degrees Celsius.
[0060] The modifier for fiber treatment and the modification method thereof in the seco...
Embodiment 3
[0061] Embodiment 3, the modifying agent for fiber treatment is prepared from the following raw materials, specifically:
[0062] N-methylolacrylamide 20% (owf);
[0063] Zinc chloride 12;
[0064] The bath ratio is 1:20.
[0065] Wherein, the modifying agent for fiber treatment in the third embodiment can modify the fiber material according to the following modification method. Specifically, the fiber modification method includes the following process steps:
[0066] a. Put the modifier in clear water to obtain a modifier solution. The modifier is prepared from the following raw materials, specifically:
[0067] N-methylolacrylamide 20% (owf);
[0068] Zinc chloride 12g / L;
[0069] Bath ratio 1:20;
[0070] b. Soak the fiber material in the modifier solution for 10 minutes;
[0071] c. After the fiber material is soaked, dry the fiber material at a temperature of 90 degrees Celsius.
[0072] The modifier for fiber treatment and the modification method thereof in the th...