A flexible ultraviolet detector and method for obtaining a GaN nanorod array grown on a graphene substrate by a non-destructive transfer process
By growing GaN nanopillar arrays on graphene substrates and performing damage-free transfer, we solve the problem of growing high-performance GaN one-dimensional nanoarrays on flexible substrates, achieve efficient preparation of flexible UV detectors, and improve photoelectric response performance and shape. Appearance integrity.
Patent Information
- Application Number
- CN201911056975.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-10-31
AI Technical Summary
It is difficult to grow high-performance GaN one-dimensional nanoarray-based devices on flexible substrates with existing technology, which limits the development of flexible or wearable applications.
A GaN nanocolumn array is grown on a graphene substrate, and a GaN nanocolumn array/graphene/substrate structure is formed on the graphene surface through PA-MBE equipment. Combined with PMMA spin coating and wet etching processes, the GaN nanocolumn array is realized. Damage-free transfer to a flexible substrate to form a flexible UV detector.
The preparation of flexible ultraviolet detectors with simple process, low energy consumption, time saving and high efficiency is realized, ensuring the morphological integrity and flexible bending ability of the GaN nanopillar array, improving the photoelectric response sensitivity and the transparency of the detector.
Smart Images

Figure CN110690312B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ultraviolet detectors, and in particular relates to a flexible ultraviolet detector and a method for obtaining the same by a damage-free transfer process of a GaN nanocolumn array grown on a graphene substrate. Background Art
[0002] Flexible, bendable, and convenient semiconductor optoelectronic devices, with their light weight, flexibility, intelligence, and efficiency, will bring about changes in the future of smart wearables, curved displays, and implantable devices. Among the many optoelectronic devices, UV light switches or photodetectors, as indispensable components of photoelectric sensors, have great application potential in various fields such as visible light communications, industrial automatic control, and ultraviolet infrared imaging, and have received special attention from many researchers around the world in the past few decades.
[0003] Currently, the use of low-dimensional wide-bandgap semiconductor nanomaterials, such as GaN, ZnO, and other metal oxide nanostructures, to develop flexible UV light switches or photodetectors with highly enhanced responsiveness and photoconductive gain has attracted strong research attention. Among them, GaN one-dimensional nanoarray materials have become a hot topic in recent years due to their unique nanostructure-induced quantum confinement effects, such as enhanced carrier mobility, excellent light absorption / emission, and almost zero dislocation density. On the one hand, the huge surface-to-volume ratio of one-dimensional nanopillars significantly increases light absorption and improves the density of photogenerated carriers. On the other hand, the low-dimensional nanostructure limits the active area of charge carriers and shortens the carrier transmission time.
[0004] Although GaN one-dimensional nanoarrays have great potential, high-performance GaN one-dimensional nanoarray-based devices are often prepared on rigid non-flexible substrates (such as sapphire, silicon, LiAlO2, MgO, etc.). This is because the epitaxial growth of such GaN one-dimensional nanoarray-based devices requires very high growth temperatures and lattice-matched single crystal substrates, while such GaN one-dimensional nanoarrays cannot be directly epitaxially grown on flexible substrates (such as PET, ITO). This limitation seriously hinders the rapidly growing demand for related flexible or wearable applications [Kuykendall, T., Pauzauskie, PJ, Zhang, Y.,Goldberger, J., Sirbuly, D., Denlinger, J. and Yang, P. Crystallographic alignment of high-density gallium nitride nanowire arrays. Nature Materials,3 (2004) 524–528. doi:10.1038 / nmat1177.]. Summary of the invention
[0005] In order to overcome the shortcomings and deficiencies of the prior art, the present invention aims to provide a non-destructive transfer process for GaN nanorod arrays grown on a graphene substrate to obtain a flexible ultraviolet detector and method. The preparation method is simple, low in energy consumption, time-saving and efficient.
[0006] The purpose of the present invention is achieved through the following technical solutions.
[0007] A flexible ultraviolet detector with a GaN nanocolumn array grown on a graphene substrate comprises, from bottom to top, a flexible substrate, a pair of interdigital electrodes on the flexible substrate, a graphene layer above the interdigital electrodes, and a GaN nanocolumn array grown on the graphene layer.
[0008] Furthermore, the flexible substrate is made of PET, PDMS, or ITO material.
[0009] Furthermore, the interdigital electrode is a layer of Au metal; the thickness of the interdigital electrode is 100-120 nm; the length of the interdigital electrode is 280-300 μm, the width is 5-15 μm, the electrode spacing is 5-20 μm, and the number of pairs is 20-24.
[0010] Furthermore, the length of the GaN nanocolumns in the GaN nanocolumn array is 300-380 nm, and the diameter is 60-80 nm; the density of the GaN nanocolumn array is 5.0×10 9 ~ 9.0×10 9 / cm 2 .
[0011] The method for preparing the flexible ultraviolet detector of the GaN nanorod array grown on the graphene substrate described above comprises the following steps:
[0012] (1) Placing the graphene substrate in a radio frequency assisted molecular beam epitaxy (PA-MBE) device, growing a GaN nanorod array on the graphene surface, and forming a GaN nanorod array / graphene / substrate structure;
[0013] (2) spin coating a layer of polymethyl methacrylate (PMMA) on the surface of the GaN nanorod array obtained in step (1) and heat curing it to form a PMMA / GaN nanorod array / graphene / substrate structure;
[0014] (3) removing the substrate layer of the structure obtained in step (2) by a wet etching process to obtain a PMMA / GaN nanorod array / graphene composite film, and transferring the PMMA / GaN nanorod array / graphene composite film to a flexible substrate coated with an interdigitated electrode structure;
[0015] (4) After the transfer in step (3), a layer of polymethyl methacrylate is spin-coated on the surface of the PMMA / GaN nanorod array / graphene / electrode flexible substrate and heated to cure, then washed with deionized water and dried, and finally the PMMA on the surface is removed and dried to obtain a flexible ultraviolet detector with a GaN nanorod array grown on a graphene substrate.
[0016] Furthermore, in step (1), the graphene is grown on a copper foil substrate by a general chemical vapor deposition (CVD) process or is grown on a SiO2 / Si substrate by a plasma enhanced chemical vapor deposition (PECVD) process.
[0017] Furthermore, in step (1), the process conditions for growing the GaN nanorod array on the graphene surface are: first, a mechanical pump and a molecular pump are used to evacuate the growth chamber until the pressure is maintained at 2×10 -9 ~4×10 -9 Torr, the substrate temperature was raised to 960-980 °C, the Ga beam current was accurately measured by ion beam equivalent pressure (BEP), and then the growth was started. The growth was divided into two steps. In the first step, H2 / N2 plasma was introduced to hydrogenate and nitride the graphene to open the CC sp 2 The second step was to stop the introduction of H2, set the N2 flow rate to 2.0-2.2 sccm, and set the RF plasma power to 360-380 W. Then, the Ga source beam was turned on, and the Ga-BEP was set to 6.5×10 -8 ~7.5×10 -8 Torr, and the total growth time was 4.0~4.5 h.
[0018] Furthermore, in step (2), the PMMA spin coating process is as follows: placing the GaN nanorod array / graphene / substrate structure obtained in step (1) on the turntable of a coating machine, coating the surface with a 1.6-1.8wt% PMMA solution, and setting two-step rotation speeds: low speed 400-500 rpm, 5-6 s; high speed 3500-4000 rpm, 28-30 s; the heating and curing process is as follows: heating temperature 140-150°C, heating time 2-3 min, so as to make it cure quickly.
[0019] Furthermore, in step (3), the process of removing the substrate layer of the structure obtained in step (2) by a wet etching process is as follows: if the graphene is grown on a copper foil substrate by a general chemical vapor deposition process, the copper foil is etched using a 0.05-0.06 g / ml ferric nitrate solution for 10-12 h; if the graphene is grown on a SiO2 / Si substrate by a plasma enhanced chemical vapor deposition process, the silicon dioxide is etched using a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:6-7 (volume ratio)) for 30-45 min.
[0020] Furthermore, in step (4), the PMMA spin coating process is as follows: placing the PMMA / GaN nanorod array / graphene / electrode flexible substrate transferred in step (3) on the turntable of a coating machine, coating the surface with a 1.6-1.8wt% PMMA solution, and setting two-step rotation speeds: low speed 400-500 rpm, 5-6 s; high speed 3500-4000 rpm, 28-30 s; the heating and curing process is as follows: heating temperature 95-100 °C, heating time 120-180 min, so that it is slowly cured, so that the stress inside the first layer of PMMA is released, and the GaN nanorod array / graphene is perfectly fitted with the electrode flexible substrate, preventing the occurrence of cracks and wrinkles.
[0021] Furthermore, in step (4), the process for removing PMMA is: immersing and cleaning in acetone for 5 to 6 times, each time for 40 to 60 seconds, to remove any residual PMMA.
[0022] Compared with the prior art, it has the following advantages and beneficial effects:
[0023] (1) The present invention discloses a method for obtaining a flexible ultraviolet detector by a non-destructive transfer process of a GaN nanorod array grown on a graphene substrate. The method has the characteristics of simple process, time-saving, high efficiency and low energy consumption, and is conducive to large-scale production.
[0024] (2) The transfer process provided by the present invention uses a two-step PMMA spin coating process, so that the stress inside the PMMA is released, and the GaN nanocolumn array / graphene is perfectly fitted with the electrode flexible substrate, preventing the appearance of cracks and wrinkles. The morphology of the GaN nanocolumn array after transfer is almost unchanged from that before transfer, and it can be flexibly bent. The transfer process is completely damage-free.
[0025] (3) The non-destructive transfer process of the GaN nanorod array grown on the graphene substrate of the present invention obtains a flexible ultraviolet detector. On the one hand, it utilizes the transparent, conductive and flexible characteristics of the graphene / GaN nanorod array material to improve the detector's light collection and photoelectric response sensitivity; on the other hand, it utilizes the huge specific surface area and quantum confinement of the one-dimensional nanorod material to increase the density and transmission time of photogenerated carriers.
[0026] (4) The present invention realizes the transparency and flexibility of the ultraviolet detector, which can be used in the fields of smart wearables, curved displays, flexible sensing imaging, etc., with considerable economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A roadmap for the method of obtaining a flexible UV detector by a damage-free transfer process of a GaN nanorod array grown on a graphene substrate of the present invention.
[0028] Figure 2 The present invention is a schematic structural diagram of each step of obtaining a flexible ultraviolet detector according to the method of the present invention; the numbers in the figure are: 1-copper foil substrate or SiO2 / Si substrate; 2-graphene; 3-GaN nanocolumn array; 4-PMMA; 5-metal Au electrode; 6-flexible substrate.
[0029] Figure 3a , Figure 3b These are SEM electron microscope photographs of the surface of the GaN nanorod array before and after transfer in Example 1.
[0030] Figure 4 This is a curve diagram showing the change of the current I of the flexible ultraviolet detector of Example 1 with the applied bias voltage V.
[0031] Figure 5 The schematic diagram of the structure of the flexible ultraviolet detector of the present invention is a GaN nanocolumn array grown on a graphene substrate. DETAILED DESCRIPTION
[0032] The present invention will be further described in detail below in conjunction with specific embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0033] In the following specific embodiments, the roadmap of the method for obtaining a flexible ultraviolet detector by a non-destructive transfer process of a GaN nanorod array grown on a graphene substrate is as follows: Figure 1 The structural schematic diagram of each step of the method of the present invention to obtain a flexible ultraviolet detector is shown in FIG. Figure 2As shown, structure A is a GaN nanocolumn array / graphene / substrate structure, structure B is a PMMA / GaN nanocolumn array / graphene / substrate structure, structure C is a PMMA / GaN nanocolumn array / graphene composite film, and structure D is a GaN nanocolumn array / graphene flexible ultraviolet detector. The structural schematic diagram of the flexible ultraviolet detector of the GaN nanocolumn array grown on the graphene substrate of the present invention is shown in FIG. Figure 5 As shown, from bottom to top, it includes a flexible substrate 6, a pair of interdigital electrodes 5 on the flexible substrate, a graphene layer 2 above the interdigital electrodes, and a GaN nanocolumn array 3 grown on the graphene layer 2.
[0034] Example 1
[0035] A method for obtaining a flexible ultraviolet detector by a non-destructive transfer process of a GaN nanorod array grown on a graphene substrate comprises the following steps:
[0036] (1) The graphene substrate is placed in a PA-MBE device and a GaN nanocolumn array is grown on the graphene surface to form a GaN nanocolumn array / graphene / substrate structure.
[0037] (2) Spin coating a layer of PMMA on the surface of the GaN nanorod array and heat curing it to form a PMMA / GaN nanorod array / graphene substrate structure.
[0038] (3) Using a wet etching process to remove the substrate layer of the structure obtained in step (2), a PMMA / GaN nanorod array / graphene composite film is obtained, and the composite film is transferred to a PET flexible substrate coated with an electrode structure.
[0039] (4) Spin-coating a layer of PMMA on the surface of the transferred PMMA / GaN nanorod array / graphene / electrode PET flexible substrate and heating and curing it, then washing it with deionized water and drying it. Finally, removing the PMMA on the surface and drying it to obtain a flexible UV detector with a GaN nanorod array grown on a graphene substrate.
[0040] In step (1), the graphene is grown on a copper foil substrate by a general CVD process or grown on a SiO2 / Si substrate by a PECVD process.
[0041] In step (1), the process conditions for the PA-MBE growth of GaN nanorod arrays are as follows: first, a mechanical pump and a molecular pump are used to evacuate the growth chamber until the pressure is maintained at 2×10 -9Torr, the substrate temperature rises to 980 °C, and the Ga beam current is accurately measured by BEP. The growth begins, and the growth is divided into two steps: the first step is to introduce H2 / N2 plasma to hydrogenate and nitride the graphene, in order to open the CC sp 2 In the first step, the H2 / N2 flow rate was set to 1.0 / 2.5 sccm, and the RF plasma power was set to 400 W. In the second step, the H2 was stopped, the N2 flow rate was set to 2.0 sccm, and the RF plasma power was set to 380 W. Then, the Ga source beam was turned on, and the Ga-BEP was set to 7.5×10 -8 Torr, and the total growth time was 4.0 h.
[0042] In step (1), the length of the GaN nanocolumns in the grown GaN nanocolumn array is 300 nm and the diameter is 80 nm; the density of the GaN nanocolumns is 7.6×10 9 / cm 2 .
[0043] In step (2) and step (4), the PMMA spin coating process is as follows: the GaN nanorod array / graphene / substrate structure obtained in step (1) is placed on the turntable of a coating machine, 1.6 wt% PMMA solution is coated on the surface, and two rotation speeds are set: low speed 400 rpm, 6 s; high speed 3500 rpm, 30 s.
[0044] In step (2), the heating curing process is: heating temperature 140 ° C, 2 min, so as to achieve rapid curing.
[0045] In step (3), the wet etching process for removing the substrate layer is as follows: if the substrate is grown on a copper foil substrate by CVD, the copper foil is etched with a 0.05 g / ml ferric nitrate solution for 12 h; if the substrate is grown on a SiO2 / Si substrate by PECVD, the silicon dioxide is etched with a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:6 (volume ratio)) for 45 min.
[0046] In step (3), the electrodes plated on the PET flexible substrate are Au metal interdigital electrodes with a thickness of 100 nm, a length of 280 μm, a width of 5 μm, an electrode spacing of 20 μm, and a pair number of 24.
[0047] In step (4), the heating and curing process is: heating temperature 95 ° C, 180 min, so that it is slowly cured, so that the stress inside the first layer of PMMA is released, and the GaN nanorod array / graphene is perfectly fitted with the electrode flexible substrate to prevent the occurrence of cracks and wrinkles.
[0048] In step (4), the PMMA removal process is: immersion cleaning in acetone 5 times, each time for 60 s, to remove any residual PMMA.
[0049] The surface electron microscope photos of the GaN nanorod array grown on the graphene substrate in this embodiment before and after transfer are shown in FIG. Figure 3a , Figure 3b As shown, from Figure 3b It can be clearly seen that the morphology of the GaN nanorod array after transfer is different from that before transfer ( Figure 3a ) has almost no major change and can be bent flexibly, proving that the transfer process is completely damage-free.
[0050] The curve diagram of the current I of the PET flexible ultraviolet detector obtained in this embodiment changing with the applied bias voltage V is shown in FIG. Figure 4 As shown in the figure, the current increases with the increase of the applied bias voltage, basically showing a typical Schottky contact pattern. In the absence of light, the dark current at 1V bias is only 0.14 nA. Under 365 nm light irradiation, the photocurrent at 1V bias is 15.2 μA, and the current increases significantly, indicating good photoelectric response performance.
[0051] Example 2
[0052] A method for obtaining a flexible ultraviolet detector by a non-destructive transfer process of a GaN nanorod array grown on a graphene substrate comprises the following steps:
[0053] (1) The graphene substrate is placed in a PA-MBE device and a GaN nanocolumn array is grown on the graphene surface to form a GaN nanocolumn array / graphene / substrate structure.
[0054] (2) Spin coating a layer of PMMA on the surface of the GaN nanorod array and heat curing it to form a PMMA / GaN nanorod array / graphene substrate structure.
[0055] (3) The substrate layer of the structure obtained in step (2) is removed by a wet etching process to obtain a PMMA / GaN nanorod array / graphene composite film, which is then transferred to a PDMS flexible substrate coated with an electrode structure.
[0056] (4) Spin-coat another layer of PMMA on the surface of the transferred PMMA / GaN nanorod array / graphene / electrode PDMS flexible substrate and heat-cure it, then wash it in deionized water, dry it, and finally remove the PMMA on the surface and dry it to obtain a flexible UV detector with a GaN nanorod array grown on a graphene substrate.
[0057] In step (1), the graphene is grown on a copper foil substrate by a general CVD process or grown on a SiO2 / Si substrate by a PECVD process.
[0058] In step (1), the process conditions for the PA-MBE growth of GaN nanorod arrays are as follows: first, a mechanical pump and a molecular pump are used to evacuate the growth chamber until the pressure is maintained at 3×10 -9 Torr, the substrate temperature rises to 960 °C, and the Ga beam current is accurately measured by BEP. The growth begins, and the growth is divided into two steps: the first step is to introduce H2 / N2 plasma to hydrogenate and nitride the graphene, in order to open the CC sp 2 bond to provide more nucleation sites for 3.5 min, the H2 / N2 flow rate was set to 1.2 / 2.8 sccm, and the RF plasma power was 395 W. In the second step, the H2 was stopped, the N2 flow rate was set to 2.2 sccm, the RF plasma power was set to 360 W, and then the Ga source beam was turned on, and the Ga-BEP was set to 7.0×10 -8 Torr, and the total growth time was 4.5 h.
[0059] In step (1), the length of the GaN nanocolumns in the grown GaN nanocolumn array is 380 nm and the diameter is 70 nm; the density of the GaN nanocolumns is 9.0×10 9 / cm 2 .
[0060] In steps (2) and (4), the PMMA spin coating process is as follows: the GaN nanorod array / graphene / substrate structure obtained in step (1) is placed on the turntable of a coating machine, 1.8% PMMA solution is coated on the surface, and two-step rotation speed is set: low speed 500 rpm, 6 s; high speed 4000 rpm, 28 s.
[0061] In step (2), the heating curing process is: heating temperature 145 ° C, 2.5 min, so as to achieve rapid curing.
[0062] In step (3), the wet etching process for removing the substrate layer is as follows: if the substrate is grown on a copper foil substrate by CVD, the copper foil is etched with a 0.056 g / ml ferric nitrate solution for 11 h; if the substrate is grown on a SiO2 / Si substrate by PECVD, the silicon dioxide is etched with a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:7 (volume ratio)) for 30 min.
[0063] In step (3), the electrodes plated on the PDMS flexible substrate are Au metal interdigital electrodes with a thickness of 120 nm, a length of 300 μm, a width of 10 μm, an electrode spacing of 15 μm, and a pair number of 20.
[0064] In step (4), the heating and curing process is: heating temperature 100 ° C, 120 min, so that it is slowly cured, so that the stress inside the first layer of PMMA is released, and the GaN nanorod array / graphene is perfectly fitted with the electrode flexible substrate to prevent the occurrence of cracks and wrinkles.
[0065] In step (4), the PMMA removal process is: immersion cleaning in acetone 6 times, each time for 40 s, to remove any residual PMMA.
[0066] The surface electron microscope photos of the GaN nanorod array grown on the graphene substrate before and after the transfer in this example are shown in FIG. Figure 3a , Figure 3b .
[0067] Example 3
[0068] A method for obtaining a flexible ultraviolet detector by a non-destructive transfer process of a GaN nanorod array grown on a graphene substrate comprises the following steps:
[0069] (1) The graphene substrate is placed in a PA-MBE device and a GaN nanocolumn array is grown on the graphene surface to form a GaN nanocolumn array / graphene / substrate structure.
[0070] (2) Spin coating a layer of PMMA on the surface of the GaN nanorod array and heat curing it to form a PMMA / GaN nanorod array / graphene substrate structure.
[0071] (3) removing the substrate layer of the structure obtained in step (2) by a wet etching process to obtain a PMMA / GaN nanorod array / graphene composite film, and transferring it to an ITO flexible substrate coated with an electrode structure.
[0072] (4) Spin-coating a layer of PMMA on the surface of the transferred PMMA / GaN nanorod array / graphene / electrode ITO flexible substrate and heating and curing it, then washing it in deionized water and drying it. Finally, removing the PMMA on the surface and drying it to obtain a flexible UV detector with a GaN nanorod array grown on a graphene substrate.
[0073] In step (1), the graphene is grown on a copper foil substrate by a general CVD process or grown on a SiO2 / Si substrate by a PECVD process.
[0074] In step (1), the process conditions for the PA-MBE growth of GaN nanorod arrays are as follows: first, a mechanical pump and a molecular pump are used to evacuate the growth chamber until the pressure is maintained at 4×10 -9 Torr, the substrate temperature rises to 970 °C, and the Ga beam current is accurately measured by BEP. The growth begins, and the growth is divided into two steps: the first step is to introduce H2 / N2 plasma to hydrogenate and nitride the graphene, in order to open the CC sp 2 bond to provide more nucleation sites for 3 min, the H2 / N2 flow rate was set to 1.5 / 3.0 sccm, and the RF plasma power was 390 W. In the second step, the H2 was stopped, the N2 flow rate was set to 2.1 sccm, the RF plasma power was set to 370 W, and then the Ga source beam was turned on, and the Ga-BEP was set to 6.5×10 -8 Torr, and the total growth time was 4.3 h.
[0075] In step (1), the length of the GaN nanocolumns in the grown GaN nanocolumn array is 350 nm and the diameter is 60 nm; the density of the GaN nanocolumns is 5.0×10 9 / cm 2 .
[0076] In steps (2) and (4), the PMMA spin coating process is as follows: the GaN nanorod array / graphene / substrate structure obtained in step (1) is placed on the turntable of a coating machine, 1.7% PMMA solution is coated on the surface, and two speeds are set: low speed 450 rpm, 5.5 s; high speed 3800 rpm, 29 s.
[0077] In step (2), the heating curing process is: heating temperature 150 ° C, 3 minutes, so as to achieve rapid curing.
[0078] In step (3), the wet etching process for removing the substrate layer is as follows: if the substrate is grown on a copper foil substrate by CVD, the copper foil is etched with a 0.06 g / ml ferric nitrate solution for 10 h; if the substrate is grown on a SiO2 / Si substrate by PECVD, the silicon dioxide is etched with a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:6.5 (volume ratio)) for 40 min.
[0079] In step (3), the electrode plated on the ITO flexible substrate is an Au metal interdigital electrode with a thickness of 110 nm, a length of 290 μm, a width of 15 μm, an electrode spacing of 5 μm, and a pair number of 22.
[0080] In step (4), the heating and curing process is: heating temperature 98 ° C, 160 min, so that it is slowly cured, so that the stress inside the first layer of PMMA is released, and the GaN nanorod array / graphene is perfectly fitted with the electrode flexible substrate, preventing the occurrence of cracks and wrinkles.
[0081] In step (4), the PMMA removal process is as follows: immersion cleaning in acetone 6 times, 50 s each time, to remove any residual PMMA.
[0082] The surface electron microscope photos of the GaN nanorod array grown on the graphene substrate before and after the transfer in this example are shown in FIG. Figure 3a , Figure 3b .
[0083] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a flexible ultraviolet detector of GaN nanorod array grown on a graphene substrate, It is characterized in that The steps include: (1) Placing the graphene substrate in a radio frequency assisted molecular beam epitaxy device, growing a GaN nanocolumn array on the graphene surface, and forming a GaN nanocolumn array / graphene / substrate structure; (2) spin coating a layer of polymethyl methacrylate on the surface of the GaN nanorod array obtained in step (1) and heat curing it to form a PMMA / GaN nanorod array / graphene / substrate structure; (3) removing the substrate layer of the structure obtained in step (2) by a wet etching process to obtain a PMMA / GaN nanorod array / graphene composite film, and transferring the PMMA / GaN nanorod array / graphene composite film to a flexible substrate coated with an interdigitated electrode structure; (4) Spin-coating a layer of polymethyl methacrylate on the surface of the PMMA / GaN nanorod array / graphene / electrode flexible substrate after transfer in step (3) and heating and curing, then washing with deionized water, and then drying, and finally removing the PMMA on the surface and drying to obtain a flexible ultraviolet detector with a GaN nanorod array grown on a graphene substrate; In step (1), the process conditions for growing the GaN nanorod array on the graphene surface are: first, a mechanical pump and a molecular pump are used to evacuate the growth chamber until the pressure is maintained at 2×10 -9 ~4×10 -9 Torr, the substrate temperature was raised to 960-980 °C, the Ga beam current was accurately measured using the ion beam equivalent pressure, and then the growth was started. The growth was divided into two steps. In the first step, H 2 / N 2 The graphene was hydrogenated and nitrided by plasma for 3-4 min. 2 / N 2 The flow rate was set to (1.0~1.5) / (2.5~3.0) sccm, and the RF plasma power was 390~400 W. In the second step, the H 2 , N 2 The flow rate was set to 2.0~2.2 sccm, the RF plasma power was set to 360~380 W, and then the Ga source beam was turned on, and the Ga-BEP was set to 6.5×10 -8 ~7.5×10 -8 Torr, and the total growth time was 4.0~4.5 h.
2. The method according to claim 1, It is characterized in that In step (1), the graphene is grown on a copper foil substrate by a general chemical vapor deposition process or grown on a SiO substrate by a plasma enhanced chemical vapor deposition process. 2 / Si substrate.
3. The method according to claim 1, It is characterized in that In step (2), the PMMA spin coating process is as follows: placing the GaN nanorod array / graphene / substrate structure obtained in step (1) on the turntable of a coating machine, coating the surface with a 1.6-1.8wt% PMMA solution, and setting two-step rotation speeds: low speed 400-500 rpm, 5-6 s; high speed 3500-4000 rpm, 28-30 s; the heating and curing process is as follows: heating temperature 140-150°C, heating time 2-3 min.
4. The method according to claim 1, It is characterized in that In step (3), the process of removing the substrate layer of the structure obtained in step (2) by wet etching is as follows: if the graphene is grown on a copper foil substrate by a general chemical vapor deposition process, the copper foil is etched with a 0.05-0.06 g / ml ferric nitrate solution for 10-12 h; if the graphene is grown on a SiO substrate by a plasma enhanced chemical vapor deposition process, the copper foil is etched with a 0.05-0.06 g / ml ferric nitrate solution for 10-12 h; 2 If the SiO2 is grown on a Si / Si substrate, BOE buffered etching solution is used to etch the SiO2 for 30 to 45 min.
5. The method according to claim 1, Features: In step (3), the interdigital electrode is a layer of Au metal; the thickness of the interdigital electrode is 100-120 nm; the length of the interdigital electrode is 280-300 μm, the width is 5-15 μm, the electrode spacing is 5-20 μm, and the number of pairs is 20-24.
6. The method according to claim 1, It is characterized in that In step (4), the PMMA spin coating process is as follows: placing the PMMA / GaN nanorod array / graphene / electrode flexible substrate transferred in step (3) on the turntable of a coating machine, coating the surface with a 1.6-1.8wt% PMMA solution, and setting two-step rotation speeds: low speed 400-500 rpm, 5-6 s; high speed 3500-4000 rpm, 28-30 s; the heating and curing process is as follows: heating temperature 95-100°C, heating time 120-180 min.
7. The method according to claim 1, It is characterized in that In step (4), the process for removing PMMA is: immersing and cleaning in acetone for 5 to 6 times, each time for 40 to 60 seconds.
Citation Information
Patent Citations
HEMT with integrated ordered GaN-base nanowire array and preparation method thereof
CN105118860A
Flexible optoelectronic device based on graphene and II-VI group semiconductor axial p-n junction nanowire array and preparation method thereof
CN105304729A
GaN nano column grown epitaxially on silicon / graphene composite substrate and preparation method thereof
CN109003888A
InGaN nano-pillar array based GSG type tunable photodetector and preparation method thereof
CN110246913A
And flexible ultraviolet detector grows on GaN nano column array on graphene substrate
CN210805800U