A self-powered ultraviolet detector based on single-layer MoS2 film / GaN nanorod array and its preparation method
By growing a single-layer MoS2 film on a GaN nanopillar array and utilizing the photovoltaic effect of the MoS2/GaN heterojunction, the problem of insufficient response performance of existing self-powered ultraviolet detectors is solved, and a self-powered self-powered device with high sensitivity and ultra-fast response is achieved. function, reducing device size and cost, and the process is efficient and low energy consumption.
Patent Information
- Application Number
- CN201911056006.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-10-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2039-10-31
AI Technical Summary
The self-powered photoelectric response performance of existing self-powered ultraviolet detectors is insufficient, and there are problems with external power supply in integrated applications, resulting in high device volume and cost.
A self-powered UV detector based on a single-layer MoS2 film/GaN nanocolumn array is used. By growing a single-layer MoS2 film on the GaN nanocolumn array and utilizing the photovoltaic effect of the MoS2/GaN heterojunction, the self-powered function is achieved, combined with high efficiency. The process preparation method includes PA-MBE and spin coating wet transfer process to form a patterned structure.
It achieves high sensitivity and ultra-fast ultraviolet light response, reduces device size and volume, improves the application prospects of optoelectronic integrated devices, and has simple process and low energy consumption.
Smart Images

Figure CN110690317B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of ultraviolet detectors, and in particular relates to a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanocolumn array and a preparation method thereof. Background Art
[0002] Ultraviolet detection technology is widely used in military and civilian facilities such as flame detection, ozone hole monitoring, ultraviolet communication, national defense early warning and tracking. In today's highly integrated electronic equipment, ultraviolet detectors, as important photoelectric conversion devices, have become an inevitable trend of miniaturization and integration.
[0003] The third generation wide bandgap semiconductor material GaN, with a bandgap of 3.4 eV, is an ideal raw material for ultraviolet detectors. In order to further reduce cost and volume, improve performance, and achieve the level of optoelectronic integrated application, the use of one-dimensional nanostructured GaN as an ultraviolet detector has become a hot topic in recent years. The advantages of one-dimensional GaN nanostructured ultraviolet detectors are as follows: its crystal quality is better than that of thin films, because the one-dimensional nanostructure is almost completely relaxed, which can effectively reduce the dislocations penetrating to the top of the nanorod, help reduce defects and improve crystal quality; in addition, the one-dimensional GaN nanostructure greatly increases the sidewall area of the material, thereby increasing the photon escape / absorption angle, effectively improving light emission / absorption, and thus improving the detector performance. However, to make this nano optoelectronic integrated system, that is, the integration of multiple nanodevices possible, these nanodevices must be self-sufficient, that is, they do not require external power to operate, because external power will greatly increase the size and weight of the device system. The key to overcoming this problem is to use self-powered ultraviolet detectors. It uses the photovoltaic effect (PV) in the device structure, that is, electron-hole pairs are generated in the semiconductor under light, and are effectively separated under the action of the built-in electric field formed by the device's own pn junction, Schottky junction or heterojunction to generate photocurrent. In this case, the device is classified as a PV (or self-powered) photodetector. At present, there have been many research reports on GaN self-powered UV detectors based on pn junctions and Schottky junctions. However, the self-powered photoelectric response performance of such self-powered UV detectors needs to be improved. Therefore, in order to obtain high-performance self-powered UV detectors based on heterojunctions [Bie, Y. , Liao, Z. ,Zhang, H. , Li, G. , Ye, Y. , Zhou, Y. , Xu, J. , Qin, Z. , Dai, L. and Yu,D., Self-Powered, Ultrafast, Visible-Blind UV Detection and Optical LogicalOperation based on ZnO / GaN Nanoscale p-n Junctions. Advanced Materials, 23(2011) 649-653. doi:10.1002 / adma.201003156], it is very important to construct a heterojunction of two different materials with matched lattices and energy bands.
[0004] As an emerging nanomaterial system, graphene-like two-dimensional layered materials are widely used in various photodetectors working in different spectral regions. Molybdenum disulfide (MoS2) is the most popular two-dimensional layered material currently studied. Single-layer MoS2 film is a new type of two-dimensional semiconductor material. The quantum confinement characteristics of its two-dimensional structure and strong bound excitons make its light absorption performance very excellent. Literature reports that the absorption coefficient in the visible light band is as high as 5×10 7 m -1 In addition, the single-layer MoS2 film has extremely high electron mobility and ultra-fast photoelectric response, which makes it very suitable for the preparation of photodetectors. However, there are no reports on ultraviolet detectors combining it with one-dimensional GaN nanostructures, so it has great development prospects. Summary of the invention
[0005] In order to overcome the shortcomings and deficiencies of the prior art, the present invention aims to provide a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array and a preparation method thereof. The preparation method has simple process, low energy consumption, time saving and high efficiency.
[0006] The purpose of the present invention is achieved by at least one of the following technical solutions.
[0007] A self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanocolumn array comprises, from bottom to top, a substrate, a GaN nanocolumn array, and a single-layer MoS2 film; the single-layer MoS2 film is self-supported on the top of the GaN nanocolumn array; a first metal electrode is provided on the single-layer MoS2 film; and a second metal electrode is provided at the bottom end of the GaN nanocolumn array.
[0008] Furthermore, the thickness of the substrate is 400-450 μm, and the substrate is selected from sapphire, Si or ScAlMgO4.
[0009] Furthermore, the length of the GaN nanocolumns in the GaN nanocolumn array is 350-450 nm, and the diameter is 50-75 nm; the thickness of the GaN merged film between the GaN nanocolumns in the GaN nanocolumn array and the substrate is 4-8 nm; the density of the GaN nanocolumns on the GaN nanocolumn array is 5.0×10 9 ~10.0×10 9 / cm 2 .
[0010] Furthermore, the thickness of the single-layer MoS2 film is 1-2 nm.
[0011] Furthermore, the first metal electrode and the second metal electrode are both a Ni metal layer and an Au metal layer stacked in sequence from bottom to top; the thicknesses of the Ni metal layer and the Au metal layer are 30-40 nm and 80-100 nm, respectively.
[0012] Furthermore, the lengths of the first metal electrode and the second metal electrode are both 200-220 μm, and the widths are both 60-80 μm; and the distance between the first metal electrode and the second metal electrode is 140-160 μm.
[0013] The above-mentioned method for preparing a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array comprises the following steps:
[0014] (1) The substrate is cleaned to remove surface residues and then placed in a radio frequency assisted molecular beam epitaxy (PA-MBE) device to grow a GaN nanorod array on the substrate surface to form a GaN nanorod array / substrate structure;
[0015] (2) transferring a single-layer MoS2 film to the top of the GaN nanocolumn array by a spin coating wet transfer process on the GaN nanocolumn array / substrate structure obtained in step (1), and performing post-transfer cleaning and drying to form a single-layer MoS2 film / GaN nanocolumn array / substrate structure;
[0016] (3) performing photolithography patterning on the single-layer MoS2 film / GaN nanocolumn array / substrate structure obtained in step (2), and then performing reactive plasma etching to remove the nanocolumns at the location of the second metal electrode, and removing the resist to obtain a patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure, the purpose of which is to deposit the second metal electrode in contact with the bottom end of the GaN nanocolumn;
[0017] (4) The patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure obtained in step (3) is subjected to photolithography processing, and then a first metal layer and a second metal layer are formed on the single-layer MoS2 film and the bottom of the GaN nanocolumn array by using an electron beam evaporation coating system, and the adhesive is removed to obtain the self-powered ultraviolet detector based on the single-layer MoS2 film / GaN nanocolumn array.
[0018] Furthermore, the process conditions for growing the GaN nanorod array on the substrate surface in step (1) are as follows: using a mechanical pump and a molecular pump to evacuate the growth chamber until the pressure is maintained at 1×10 -9 ~2×10 -9Torr, and heated to 880~900 ℃ for annealing for 20~30 min to remove surface residues; then the substrate temperature was raised to 970~990 ℃, the substrate rotation speed was 8~10 rpm, and the Ga beam current was accurately measured by ion beam equivalent pressure (BEP); then N2 plasma was introduced to nitride the substrate for 4~5 min, the N2 flow rate was set to 2.5~3.0 sccm, and the RF plasma power was 390~400 W; then the Ga source beam was turned on, and the Ga-BEP was set to 7.0~8.0×10 -8 Torr, the N2 flow rate was set to 2.0~2.2sccm, the RF plasma power was 360~380 W, and the total growth time was 3.0~3.2 h.
[0019] Furthermore, in step (2), the spin coating wet transfer process for transferring the single-layer MoS2 film to the top of the GaN nanocolumn array is as follows: the single-layer MoS2 film grown on the surface of the silicon dioxide / silicon substrate by a general CVD process is spin-coated with a PMMA solution for 25 to 30 seconds at a rotation speed of 3500 to 4000 rpm, and then dried to form a PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure; then the PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure is dissolved in a BOE buffer etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1: 6 to 7 (volume ratio)) for 10 to 12 minutes to etch silicon dioxide, so that the PMMA / single-layer MoS2 film layer is peeled off; then the PMMA / single-layer MoS2 film layer is washed in deionized water for 3 to 5 times; finally, the GaN nanocolumn array / substrate structure obtained in step (1) is scooped up with the PMMA / single-layer MoS2 film layer in deionized water, and then dried.
[0020] Furthermore, in step (2), the cleaning is performed by washing in acetone for 2 to 4 times; the drying temperature is 45 to 60° C., and the drying time is 0.8 to 1.2 h.
[0021] Furthermore, in steps (3) and (4), the photolithography process is as follows: first, a negative photoresist is spin-coated using a coater for 40 to 50 seconds, followed by pre-baking (heating in an oven at 75 to 85°C for 1 to 1.5 minutes), exposure to a UV light source for 5.5 to 6.0 seconds, development (dissolution in a developer for 45 to 50 seconds), and reactive ion etching using O2 plasma for 1.5 to 2.0 minutes, cleaning, and finally drying with hot nitrogen for 3 to 5 minutes.
[0022] Furthermore, in steps (3) and (4), the degumming is performed by soaking in acetone for 20 to 22 minutes and then ultrasonically treating for 30 to 40 seconds, thereby removing unnecessary parts and leaving the desired pattern.
[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0024] (1) The present invention provides a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanocolumn array, and the preparation method has the characteristics of simple process, time-saving, high efficiency and low energy consumption.
[0025] (2) The self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanocolumn array of the present invention utilizes the photovoltaic effect of the MoS2 / GaN heterojunction to prepare a self-powered ultraviolet detector, which greatly reduces the size and volume of the device and has great application prospects for optoelectronic integrated devices.
[0026] (3) The present invention utilizes the huge specific surface area and quantum confinement of the GaN one-dimensional nanorod material in a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array. In addition, the two-dimensional quantum confinement, extremely high electron mobility and ultra-fast photoelectric response of the single-layer MoS2 film are utilized to enhance light absorption, increase the density and transmission time of photogenerated carriers, and obtain a highly sensitive and ultra-fast light-response ultraviolet detector.
[0027] (4) The self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanocolumn array of the present invention can achieve high-sensitivity detection of ultraviolet light and can be applied to fields such as ultraviolet missile guidance, open fire detection and solar illumination detection, with considerable economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic diagram of the structural cross-section of the self-powered ultraviolet detector based on the single-layer MoS2 film / GaN nanocolumn array of the present invention.
[0029] Figure 2a , Figure 2b This is a SEM electron microscope photograph of the GaN nanocolumn array in Example 1.
[0030] Figure 3 This is a curve diagram showing the change of the current I of the self-powered detector of Example 1 under 325 nm ultraviolet light irradiation with the external bias voltage V. DETAILED DESCRIPTION
[0031] The present invention will be further described in detail below in conjunction with specific embodiments and drawings, but the embodiments of the present invention are not limited thereto.
[0032] In a specific embodiment, the structural cross-sectional diagram of the self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array of the present invention is as follows: Figure 1 shown by Figure 1It can be seen that, from bottom to top, it includes a substrate 1, a GaN nanorod array 2, a single-layer MoS2 film 3, a first metal electrode 4, and a second metal electrode 5.
[0033] The substrate is sapphire, Si or ScAlMgO4, with a thickness of 400-450 μm; the GaN nanocolumn array has a length of 350-450 nm and a diameter of 50-75 nm; the thickness of the GaN merged film between the GaN nanocolumns in the GaN nanocolumn array and the substrate is 4-8 nm; the density of the GaN nanocolumns on the GaN nanocolumn array is 5.0×10 9 ~10.0×10 9 / cm 2 The single-layer MoS2 film is self-supported on the top of the GaN nanocolumn array, with a thickness of 1-2 nm. The first metal electrode and the second metal electrode are Ni metal layers and Au metal layers stacked in sequence from bottom to top, with thicknesses of 30-40 nm and 80-100 nm respectively. The length of the first metal electrode and the second metal electrode are both 200-220 μm, the width is both 60-80 μm, and the distance between the two is 140-160 μm.
[0034] Example 1
[0035] The present embodiment is a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array.
[0036] The substrate is Si with a thickness of 430 μm. The length of the GaN nanopillar array is 350 nm and the diameter is 75 nm. The thickness of the GaN merged film between the GaN nanopillars in the GaN nanopillar array and the substrate is 8 nm. The density of the GaN nanopillars on the GaN nanopillar array is 10.0×10 9 / cm 2 The single-layer MoS2 film is self-supported on the top of the GaN nanopillar array, with a thickness of 1 nm. The first metal electrode and the second metal electrode are Ni metal layers and Au metal layers stacked from bottom to top, with thicknesses of 30 nm and 80 nm respectively. The length of the first metal electrode and the second metal electrode are both 220 μm, the width is 60 μm, and the distance between them is 160 μm.
[0037] The preparation method thereof comprises the following steps:
[0038] (1) The substrate is cleaned to remove surface residues and then placed in a PA-MBE device to grow a GaN nanocolumn array on the substrate surface to form a GaN nanocolumn array / substrate structure.
[0039] (2) On the GaN nanocolumn array / substrate structure, a single-layer MoS2 film is transferred to the top of the GaN nanocolumn array by a spin coating wet transfer process, and the film is cleaned and dried after the transfer to form a single-layer MoS2 film / GaN nanocolumn array / substrate structure.
[0040] (3) The above structure is subjected to photolithography patterning, followed by reactive plasma etching to remove excess nanopillars on one side and de-resin to obtain a patterned single-layer MoS2 film / GaN nanopillar array / substrate structure for the purpose of depositing a second metal electrode in contact with the bottom of the GaN nanopillar.
[0041] (4) The patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure is subjected to photolithography processing, and then a first metal layer and a second metal layer are formed on the sample surface by using an electron beam evaporation coating system, and the resist is removed to obtain the self-powered ultraviolet detector based on the single-layer MoS2 film / GaN nanocolumn array.
[0042] In step (1), the process conditions for the PA-MBE growth of GaN nanorod arrays are: using a mechanical pump and a molecular pump to evacuate the growth chamber until the pressure is maintained at 1×10 -9 Torr, and heated to 880 °C for annealing for 30 min to remove surface residues; then the substrate temperature was raised to 990 °C, the substrate rotation speed was 10 rpm, and the Ga beam current was accurately measured using the ion beam equivalent pressure (BEP). Growth began: first, N2 plasma was introduced to nitride the substrate for 5 min, the N2 flow rate was set to 3.0 sccm, and the RF plasma power was 390 W; then the Ga source beam was turned on, and the Ga-BEP was set to 7.5×10 -8 Torr, the N2 flow rate was set to 2.0 sccm, and the RF plasma power was 380 W. The total growth time was 3.2 h.
[0043] In step (2), the spin coating wet transfer process for transferring the single-layer MoS2 film to the top of the GaN nanorod array is as follows: the single-layer MoS2 film grown on the surface of the silicon dioxide / silicon substrate by the general CVD process is spin-coated with a PMMA solution for 25 seconds at a rotation speed of 4000 rpm, and then dried; forming a PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure, then dissolving the above structure in a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:7 (volume ratio)) for 12 minutes to etch the silicon dioxide, so that the PMMA / single-layer MoS2 film layer is peeled off, and then the PMMA / single-layer MoS2 film layer is washed with deionized water for 5 times to remove any residual etching solution; finally, the GaN nanorod array / substrate structure obtained in step (1) is scooped up with the PMMA / single-layer MoS2 film layer in deionized water and placed in a vacuum drying oven for drying.
[0044] In step (2), the cleaning and drying process after transfer is as follows: the transferred PMMA / single-layer MoS2 film / GaN nanorod array / substrate structure is placed in acetone for cleaning three times to remove any residual PMMA, and the final drying temperature is 45°C and the time is 1.2 h.
[0045] In steps (3) and (4), the photolithography process is as follows: first, a negative photoresist is spin-coated for 45 seconds using a coater, followed by pre-baking (heating in an oven at 75°C for 1.5 minutes), ultraviolet light exposure for 5.5 seconds, development (dissolving in a developer for 47 seconds), and reactive ion etching using O2 plasma for 1.5 minutes, cleaning, and finally hot nitrogen drying for 5 minutes.
[0046] In steps (3) and (4), the degumming is performed by soaking in acetone for 22 min and then ultrasonically treating for 30 s, thereby removing the unnecessary parts and leaving the desired pattern.
[0047] The SEM electron microscope image of the GaN nanorod array grown on the Si substrate is shown in Figure 2a , Figure 2b As shown in the figure, it can be clearly seen that the GaN nanocolumn array has a length of 350 nm and a diameter of 75 nm. The thickness of the merged film at the bottom of the nanocolumn is 8 nm, and the density is 10.0×10 9 / cm 2 .
[0048] The curve of the current I of the self-powered UV detector based on single-layer MoS2 film / GaN nanorod array under 325 nm light irradiation versus the applied bias voltage V is shown in the figure. Figure 3Under 325 nm light irradiation, the photocurrent under 0 V bias is 0.20 μA, indicating its excellent self-powered performance and photoelectric response performance.
[0049] Example 2
[0050] The present embodiment is a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array.
[0051] The substrate is ScAlMgO4 with a thickness of 400 μm. The GaN nanopillar array has a length of 450 nm and a diameter of 50 nm. The thickness of the GaN merged film between the GaN nanopillars in the GaN nanopillar array and the substrate is 4 nm. The density of the GaN nanopillars on the GaN nanopillar array is 5.0×10 9 / cm 2 The single-layer MoS2 film is self-supported on the top of the GaN nanopillar array, with a thickness of 1.5 nm. The first metal electrode and the second metal electrode are Ni metal layers and Au metal layers stacked from bottom to top, with thicknesses of 35 nm and 90 nm respectively. The length of the first metal electrode and the second metal electrode are both 200 μm, the width is 80 μm, and the distance between them is 140 μm.
[0052] The preparation method thereof comprises the following steps:
[0053] (1) The substrate is cleaned to remove surface residues and then placed in a PA-MBE device to grow a GaN nanocolumn array on the substrate surface to form a GaN nanocolumn array / substrate structure.
[0054] (2) On the GaN nanocolumn array / substrate structure, a single-layer MoS2 film is transferred to the top of the GaN nanocolumn array by a spin coating wet transfer process, and the film is cleaned and dried after the transfer to form a single-layer MoS2 film / GaN nanocolumn array / substrate structure.
[0055] (3) The above structure is subjected to photolithography patterning, followed by reactive plasma etching to remove excess nanopillars on one side and de-resin to obtain a patterned single-layer MoS2 film / GaN nanopillar array / substrate structure for the purpose of depositing a second metal electrode in contact with the bottom of the GaN nanopillar.
[0056] (4) The patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure is subjected to photolithography processing, and then a first metal layer and a second metal layer are formed on the sample surface by using an electron beam evaporation coating system, and the resist is removed to obtain the self-powered ultraviolet detector based on the single-layer MoS2 film / GaN nanocolumn array.
[0057] In step (1), the process conditions for the PA-MBE growth of GaN nanorod arrays are: using a mechanical pump and a molecular pump to evacuate the growth chamber until the pressure is maintained at 1.5×10 -9 Torr, and heated to 900 °C for annealing for 22 min to remove surface residues; then the substrate temperature was raised to 970 °C, the substrate rotation speed was 9 rpm, and the Ga beam current was accurately measured using the ion beam equivalent pressure (BEP). Growth began: first, N2 plasma was introduced to nitride the substrate for 4 min, the N2 flow rate was set to 2.8 sccm, and the RF plasma power was 395 W; then the Ga source beam was turned on, and the Ga-BEP was set to 7.0×10 -8 Torr, the N2 flow rate was set to 2.2 sccm, and the RF plasma power was 370 W. The total growth time was 3.0 h.
[0058] In step (2), the spin coating wet transfer process for transferring the single-layer MoS2 film to the top of the GaN nanorod array is as follows: the single-layer MoS2 film grown on the surface of the silicon dioxide / silicon substrate by the general CVD process is spin-coated with a PMMA solution for 30 seconds at a rotation speed of 3500 rpm, and then dried; forming a PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure, then dissolving the above structure in a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:6 (volume ratio)) for 10 minutes to etch the silicon dioxide, so that the PMMA / single-layer MoS2 film layer is peeled off, and then the PMMA / single-layer MoS2 film layer is washed 4 times with deionized water to remove any residual etching solution; finally, the GaN nanorod array / substrate structure obtained in step (1) is scooped up with the PMMA / single-layer MoS2 film layer in deionized water and placed in a vacuum drying oven for drying.
[0059] In step (2), the cleaning and drying process after transfer is as follows: the transferred PMMA / single-layer MoS2 film / GaN nanorod array / substrate structure is placed in acetone for cleaning twice to remove any residual PMMA, and the final drying temperature is 60°C and the time is 0.8 h.
[0060] In steps (3) and (4), the photolithography process is as follows: first, a negative photoresist is spin-coated for 40 seconds using a coater, followed by pre-baking (heating in an oven at 85°C for 1 minute), exposure to a UV light source for 5.8 seconds, development (dissolution in a developer for 45 seconds), and reactive ion etching using O2 plasma for 2.0 minutes, cleaning, and finally drying with hot nitrogen for 4 minutes.
[0061] In steps (3) and (4), the degumming is performed by soaking in acetone for 20 min and then ultrasonically treating for 36 s, thereby removing the unnecessary parts and leaving the desired pattern.
[0062] The SEM electron microscope photograph of the GaN nanorod array grown on the sapphire substrate described in this embodiment is shown in FIG. Figure 2a , Figure 2b .
[0063] Example 3
[0064] The present embodiment is a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array.
[0065] The substrate is ScAlMgO4 with a thickness of 450 μm. The GaN nanopillar array is 400 nm long and 65 nm in diameter. The thickness of the GaN merged film between the GaN nanopillars in the GaN nanopillar array and the substrate is 6 nm. The density of the GaN nanopillars on the GaN nanopillar array is 8.0×10 9 / cm 2 The single-layer MoS2 film is self-supported on the top of the GaN nanopillar array, with a thickness of 2 nm. The first metal electrode and the second metal electrode are Ni metal layers and Au metal layers stacked from bottom to top, with thicknesses of 40 nm and 100 nm respectively. The length of the first metal electrode and the second metal electrode are both 210 μm, the width is 70 μm, and the distance between them is 150 μm.
[0066] The preparation method thereof comprises the following steps:
[0067] (1) The substrate is cleaned to remove surface residues and then placed in a PA-MBE device to grow a GaN nanocolumn array on the substrate surface to form a GaN nanocolumn array / substrate structure.
[0068] (2) On the GaN nanocolumn array / substrate structure, a single-layer MoS2 film is transferred to the top of the GaN nanocolumn array by a spin coating wet transfer process, and the film is cleaned and dried after the transfer to form a single-layer MoS2 film / GaN nanocolumn array / substrate structure.
[0069] (3) The above structure is subjected to photolithography patterning, followed by reactive plasma etching to remove excess nanopillars on one side and de-resin to obtain a patterned single-layer MoS2 film / GaN nanopillar array / substrate structure for the purpose of depositing a second metal electrode in contact with the bottom of the GaN nanopillar.
[0070] (4) The patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure is subjected to photolithography processing, and then a first metal layer and a second metal layer are formed on the sample surface by using an electron beam evaporation coating system, and the resist is removed to obtain the self-powered ultraviolet detector based on the single-layer MoS2 film / GaN nanocolumn array.
[0071] In step (1), the process conditions for the PA-MBE growth of GaN nanorod arrays are: using a mechanical pump and a molecular pump to evacuate the growth chamber until the pressure is maintained at 2×10 -9 Torr, and heated to 890 °C for annealing for 20 min to remove surface residues; then the substrate temperature was raised to 980 °C, the substrate rotation speed was 8 rpm, and the Ga beam current was accurately measured by ion beam equivalent pressure (BEP). Growth began: first, N2 plasma was introduced to nitride the substrate for 4.5 min, the N2 flow rate was set to 2.5 sccm, and the RF plasma power was 400 W; then the Ga source beam was turned on, and the Ga-BEP was set to 8.0×10 -8 Torr, the N2 flow rate was set to 2.1 sccm, and the RF plasma power was 360 W. The total growth time was 3.1 h.
[0072] In step (2), the spin coating wet transfer process for transferring the single-layer MoS2 film to the top of the GaN nanorod array is as follows: the single-layer MoS2 film grown on the surface of the silicon dioxide / silicon substrate by the general CVD process is spin-coated with a PMMA solution for 28 seconds at a rotation speed of 3800 rpm, and then dried; forming a PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure, then dissolving the above structure in a BOE buffered etching solution (49% HF aqueous solution: 40% NH4F aqueous solution = 1:6.5 (volume ratio)) for 11 minutes to etch the silicon dioxide, so that the PMMA / single-layer MoS2 film layer is peeled off, and then the PMMA / single-layer MoS2 film layer is washed three times with deionized water to remove any residual etching solution; finally, the GaN nanorod array / substrate structure obtained in step (1) is scooped up with the PMMA / single-layer MoS2 film layer in deionized water and placed in a vacuum drying oven for drying.
[0073] In step (2), the cleaning and drying process after transfer is as follows: the transferred PMMA / single-layer MoS2 film / GaN nanorod array / substrate structure is placed in acetone for cleaning 4 times to remove any residual PMMA, and the final drying temperature is 50°C and the time is 1.0 h.
[0074] In steps (3) and (4), the photolithography process is as follows: first, negative photoresist is spin-coated for 50 seconds using a coater, followed by pre-baking (heating in an oven at 80°C for 1.2 minutes), ultraviolet light exposure for 6.0 seconds, development (dissolving in a developer for 50 seconds), and reactive ion etching using O2 plasma for 1.8 minutes, cleaning, and finally hot nitrogen drying for 3 minutes.
[0075] In steps (3) and (4), the degumming is performed by soaking in acetone for 21 min and then ultrasonically treating for 40 s, thereby removing the unnecessary parts and leaving the desired pattern.
[0076] The SEM electron microscope photograph of the GaN nanorod array grown on the ScAlMgO4 substrate described in this embodiment is shown in FIG. Figure 2a , Figure 2b .
[0077] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanorod array, characterized in that: The steps include: (1) cleaning the substrate to remove surface residues and then placing it in a radio frequency assisted molecular beam epitaxy device to grow a GaN nanorod array on the surface of the substrate to form a GaN nanorod array / substrate structure; (2) transferring a single-layer MoS2 film to the top of the GaN nanocolumn array by a spin coating wet transfer process on the GaN nanocolumn array / substrate structure obtained in step (1), and performing post-transfer cleaning and drying to form a single-layer MoS2 film / GaN nanocolumn array / substrate structure; (3) performing photolithography patterning on the single-layer MoS2 film / GaN nanocolumn array / substrate structure obtained in step (2), and then performing reactive plasma etching to remove the nanocolumns at the location of the second metal electrode, and removing the glue to obtain a patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure, the purpose of which is to deposit the second metal electrode in contact with the bottom end of the GaN nanocolumn; (4) performing photolithography on the patterned single-layer MoS2 film / GaN nanocolumn array / substrate structure obtained in step (3), and then using an electron beam evaporation coating system to evaporate and deposit a first metal layer and a second metal layer on the single-layer MoS2 film and the bottom of the GaN nanocolumn array, and removing the glue to obtain the self-powered ultraviolet detector based on the single-layer MoS2 film / GaN nanocolumn array; The self-powered ultraviolet detector based on a single-layer MoS2 film / GaN nanocolumn array comprises, from bottom to top, a substrate (1), a GaN nanocolumn array (2), and a single-layer MoS2 film (3); the single-layer MoS2 film (3) is self-supported on the top of the GaN nanocolumn array (2); a first metal electrode (4) is provided on the single-layer MoS2 film; a second metal electrode (5) is provided at the bottom end of the GaN nanocolumn array; the length of the GaN nanocolumns in the GaN nanocolumn array (2) is 350 to 450 nm, and the diameter is 50 to 75 nm; the thickness of the GaN merged film between the GaN nanocolumns in the GaN nanocolumn array and the substrate is 4 to 8 nm; the density of the GaN nanocolumns on the GaN nanocolumn array is 5.0×10 9 ~10.0×10 9 / cm 2 .
2. The preparation method according to claim 1, characterized in that: The thickness of the substrate (1) is 400-450 μm; the substrate is selected from sapphire, Si or ScAlMgO4.
3. The preparation method according to claim 1, characterized in that: The thickness of the single-layer MoS2 film (3) is 1-2 nm.
4. The preparation method according to claim 1, characterized in that: The first metal electrode (4) and the second metal electrode (5) are both Ni metal layers and Au metal layers stacked in sequence from bottom to top; the thicknesses of the Ni metal layer and the Au metal layer are 30-40 nm and 80-100 nm respectively; the lengths of the first metal electrode (4) and the second metal electrode (5) are both 200-220 μm and the widths are both 60-80 μm; the spacing between the first metal electrode (4) and the second metal electrode (5) is 140-160 μm.
5. The preparation method according to claim 1, characterized in that: The process conditions for growing the GaN nanorod array on the substrate surface in step (1) are as follows: using a mechanical pump and a molecular pump to evacuate the growth chamber until the pressure is maintained at 1×10 -9 ~2×10 -9 Torr, and heated to 880-900°C for annealing for 20-30 min to remove surface residues; then the substrate temperature was raised to 970-990°C, and the substrate substrate rotation speed was 8-10 rpm; then N2 plasma was introduced to nitride the substrate for 4-5 min, the N2 flow rate was set to 2.5-3.0 sccm, and the RF plasma power was 390-400 W; then the Ga source beam was turned on, and the Ga-BEP was set to 7.0×10 -8 ~8.0×10 -8 Torr, N2 flow rate was set to 2.0-2.2 sccm, RF plasma power was 360-380 W, and the total growth time was 3.0-3.2 h.
6. The preparation method according to claim 1, characterized in that: In step (2), the spin coating wet transfer process for transferring the single-layer MoS2 film to the top of the GaN nanocolumn array is as follows: the single-layer MoS2 film grown on the surface of the silica / silicon substrate by a general CVD process is spin-coated with a PMMA solution for 25 to 30 seconds at a rotation speed of 3500 to 4000 rpm, and dried to form a PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure; then the PMMA / single-layer MoS2 film / silicon dioxide / silicon substrate structure is dissolved in BOE buffer etching solution for 10 to 12 minutes to etch the silica, so that the PMMA / single-layer MoS2 film layer is peeled off; then the PMMA / single-layer MoS2 film layer is washed in deionized water for 3 to 5 times; finally, the GaN nanocolumn array / substrate structure obtained in step (1) is scooped up with the PMMA / single-layer MoS2 film layer in deionized water, and then dried.
7. The preparation method according to claim 1, characterized in that: In step (2), the cleaning is performed by washing in acetone for 2 to 4 times; the drying temperature is 45 to 60° C. and the drying time is 0.8 to 1.2 h.
8. The preparation method according to claim 1, characterized in that: In step (3) and step (4), the photolithography is to first use a coating machine to spin-coat a negative photoresist for 40 to 50 seconds, then heat it in an oven at 75 to 85° C. for 1 to 1.5 minutes before baking, then expose it to a UV light source for 5.5 to 6.0 seconds, dissolve it in a developer for 45 to 50 seconds for development, and use O2 plasma for reactive ion etching for 1.5 to 2.0 minutes, clean it, and finally dry it with hot nitrogen for 3 to 5 minutes; the degumming is to soak it in acetone for 20 to 22 minutes and then ultrasonically treat it for 30 to 40 seconds.
Citation Information
Patent Citations
Method for preparing self-supporting GaN substrate material
CN107611004A
Van der Waals heterojunction photoelectric detector with periodic strain and fabrication method thereof
CN109742177A
Self-powered photoelectric detection structure based on graphene-gallium oxide phase junction, device and preparation method
CN110085688A
Self-powered ultraviolet detector based on single-layer MoS2 film / GaN nanorod array
CN210805803U
Photoconductive device based on a nanowire structure comprising a graphene
KR1020160025332A