A micro-arc oxidation device with variable cathode area and surface treatment method
By introducing a circulation tank and a lifting mechanism into the micro-arc oxidation device, partitioned micro-arc oxidation is realized, which solves the problems of low processing efficiency and energy waste of large workpieces, improves film quality and production efficiency, and simplifies the process.
Patent Information
- Application Number
- CN202111269197.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The traditional immersion micro-arc oxidation surface treatment method has low processing efficiency for large workpieces, high energy waste, poor film quality, high equipment requirements, and complex operations.
A micro-arc oxidation device with variable cathode area is designed. By setting a circulation tank, a liquid level control part and a cooling circulation mechanism below the micro-arc oxidation tank, and using a lifting mechanism to make the workpiece move at a uniform speed through the workpiece channel, a partitioned micro-arc oxidation device is realized. Arc oxidation improves film growth rate and electrolyte recycling.
It improves the production efficiency of micro-arc oxidation coatings, reduces energy consumption, simplifies the process, and prepares ceramic coatings with high hardness, uniform thickness, no ablation, no cracks, and good corrosion resistance and wear resistance.
Smart Images

Figure CN113913892B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the field of surface treatment technology, and in particular to a micro-arc oxidation device with a variable cathode area and a surface treatment method. Background Art
[0002] Micro-arc oxidation (MAO) is a metal surface treatment technology that relies on the instantaneous high temperature and high pressure generated by arc discharge to grow a functional ceramic oxide film based on the matrix metal oxide on the surface of aluminum, magnesium, titanium and other metals and their alloys through the combination of electrolyte and corresponding electrical parameters. Compared with other surface treatment technologies, the advantages of micro-arc oxidation include: first, it can strengthen the surface of the matrix metal while maintaining the inherent properties of the material, making it have excellent weather resistance; second, the production equipment is simple, the process is stable, the production efficiency is high, and various complex structural parts and batch production can be achieved; third, the film composition, structure and performance can be modulated by optimizing the process parameters, especially by strictly controlling the electrolyte composition ratio to achieve "environmentally friendly" clean production; fourth, it can combine the in-situ growth of the in-situ oxidation ceramic layer and the characteristics of the porous structure of the film layer, and its MAO+X type composite film layer has a good development trend.
[0003] At present, micro-arc oxidation surface treatment is generally immersion type, specifically, the workpiece is completely immersed in the micro-arc oxidation tank filled with electrolyte, and the workpiece, electrode and positive pole of the power supply are conductively connected, as well as the stainless steel cathode plate and the negative pole of the power supply evenly distributed in the micro-arc oxidation tank are conductively connected to form a loop, and then the electrical parameters and other process parameters are controlled to carry out surface ceramic treatment. It is more suitable for micro-arc oxidation surface treatment with small size, simple geometry and batch centralized processing, and the production efficiency is very high.
[0004] However, large workpieces or workpieces with extra-wide and extra-long dimensions will encounter the following difficulties when treated by immersion micro-arc oxidation surface treatment: First, after the large surface area workpiece is fully immersed, the arc starting time is long due to the limitation of the peak current, thereby extending the processing time of the workpiece under the same surface area, resulting in a significant reduction in production efficiency and capacity; second, the time required for arc starting is long, and the electrical energy of micro-arc oxidation is converted into thermal energy, which causes the electrolyte temperature to rise rapidly, so cooling equipment is required to cool down and keep warm to ensure that the electrolyte is within the appropriate temperature range, and excessively high electrolyte temperature will destroy the electrolyte components and service life, resulting in energy waste; third, the power capacity required for large surface area workpieces is high, and as the thickness of the film layer increases, the distributed current per unit area gradually increases, resulting in an increase in the required power capacity and auxiliary equipment power, and at the same time, the related production operations are complicated and the production efficiency is low. In addition, the film thickness uniformity generated by immersion micro-arc oxidation surface treatment is poor, and it is easy to be ablated at the edge. Summary of the invention
[0005] The purpose of the embodiments of the present application is to provide a micro-arc oxidation device and a surface treatment method with a variable cathode area, which solves the technical problems of high production equipment requirements, complex operation, low production efficiency, high energy waste and poor film quality in traditional immersion micro-arc oxidation surface treatment methods.
[0006] In order to achieve the above purpose, the technical solution of the embodiment of the present application is:
[0007] In a first aspect, an embodiment of the present application provides a micro-arc oxidation device with a variable cathode area, which includes a micro-arc oxidation tank, a circulation tank, a lifting mechanism, a cooling circulation mechanism, and a power supply mechanism;
[0008] The micro-arc oxidation tank is provided with an injection port, an outflow port and a workpiece channel, and a liquid level control component is provided at the outflow port end; the workpiece channel is located at the bottom of the micro-arc oxidation tank, and the width of the workpiece channel is greater than the width of the workpiece;
[0009] A cathode component is provided in the micro-arc oxidation tank, and the cathode components are respectively located on both sides of the workpiece channel in the width direction, and the cathode components are connected to the negative electrode of the power supply mechanism;
[0010] The lifting mechanism is provided above the micro-arc oxidation tank, and an anode component is provided on the lifting mechanism, and the anode component is connected to the positive electrode of the power supply mechanism; the lifting mechanism can drive the workpiece to move downward in the micro-arc oxidation tank and pass through the workpiece channel;
[0011] The circulation groove is provided below the micro-arc oxidation groove, and a circulation inlet and a circulation outlet are provided on the circulation groove. The cooling circulation mechanism connects the outflow port with the circulation inlet, and connects the circulation outlet with the injection port, and can cool the electrolyte flowing from the circulation outlet to the injection port.
[0012] In combination with the first aspect, as a further improvement of the micro-arc oxidation device with variable cathode area, two limit plates are provided at the bottom of the micro-arc oxidation groove, the two limit plates are respectively located on both sides of the width direction of the workpiece channel, and each of the limit plates is provided with a plurality of key grooves in the length direction.
[0013] In combination with the first aspect, as a further improvement of the micro-arc oxidation device with variable cathode area, each of the limiting plates includes a pressure plate, a sealing plate and a support plate stacked in sequence from top to bottom, and the width of the sealing plate is greater than the width of the support plate, which is greater than the width of the pressure plate.
[0014] In combination with the first aspect, as a further improvement of the micro-arc oxidation device with a variable cathode area, the cathode component includes a plurality of stainless steel cathode plates and cathode copper bars;
[0015] The plurality of stainless steel cathode plates are evenly arranged on the inner wall of the micro-arc oxidation tank and located on both sides of the width direction of the workpiece channel, and the cathode copper bar connects the plurality of stainless steel cathode plates in series.
[0016] In combination with the first aspect, as a further improvement of the micro-arc oxidation device with a variable cathode area, an insulating plate is provided at the end of each stainless steel cathode plate facing away from the inner wall of the micro-arc oxidation groove, and a accommodating cavity and a plurality of air distribution holes connected to the accommodating cavity are opened in the insulating plate, the accommodating cavity is connected to an air compression mechanism, and the plurality of air distribution holes are located at the end of the insulating plate facing away from the stainless steel cathode plate.
[0017] In combination with the first aspect, as a further improvement of the micro-arc oxidation device with variable cathode area, an overflow port is further provided on the micro-arc oxidation tank, and the overflow port is located at the notch of the micro-arc oxidation tank.
[0018] In a second aspect, an embodiment of the present application further provides a micro-arc oxidation surface treatment system with a variable cathode area, which includes the above-mentioned micro-arc oxidation device with a variable cathode area and a first cleaning unit, a second cleaning unit and a drying unit;
[0019] The first cleaning unit, the micro-arc oxidation device with variable cathode area, the second cleaning unit and the drying unit are connected in sequence.
[0020] In a third aspect, the present application also provides a micro-arc oxidation surface treatment method with a variable cathode area, comprising the following steps:
[0021] Cleaning workpieces;
[0022] Using the micro-arc oxidation device with variable cathode area to perform micro-arc oxidation on the cleaned workpiece;
[0023] Cleaning workpieces after micro-arc oxidation;
[0024] Dry the workpiece.
[0025] In combination with the third aspect, as a further improvement of the micro-arc oxidation surface treatment method with variable cathode area, the micro-arc oxidation electrolyte includes 10 g / L sodium silicate, 10 g / L sodium fluoride or potassium fluoride, 10 g / L sodium hydroxide or potassium hydroxide and the remainder water.
[0026] In a fourth aspect, the embodiments of the present application also provide an application of a micro-arc oxidation surface treatment method with a variable cathode area in the manufacture of ceramic oxide film layers and alloy plates.
[0027] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present application include at least:
[0028] The micro-arc oxidation device with variable cathode area provided in the embodiment of the present application is provided with a circulation groove capable of circulating electrolyte below the micro-arc oxidation groove, and a liquid level control component and a cooling circulation mechanism are provided at the outflow end of the micro-arc oxidation groove, and a lifting mechanism capable of driving the workpiece to move downward at a uniform speed is provided above the micro-arc oxidation groove, and a workpiece channel is provided at the bottom of the micro-arc oxidation groove, as well as an anode component connected to the positive electrode of the power supply mechanism on the lifting mechanism and cathode components connected to the negative electrode of the power supply mechanism are provided on both sides of the workpiece channel in the micro-arc oxidation groove in the width direction. In view of this, the lifting mechanism is turned on to drive the workpiece to immerse in the electrolyte at a uniform speed and then pass through the workpiece channel, realizing the zoned micro-arc oxidation of the workpiece surface. On the one hand, it can be used for micro-arc oxidation surface treatment of large workpieces, and the workpiece does not need to be completely immersed in the electrolyte at one time, which improves the growth rate of the micro-arc oxidation film layer and shortens the processing cycle, thereby improving the production efficiency of the micro-arc oxidation film layer, and realizing the recycling of the electrolyte, reducing production energy consumption; on the other hand, the quality of the ceramic film layer can be controlled by controlling the dynamic parameters of the lifting mechanism and the static parameters of the micro-arc oxidation tank, so that the ceramic film layer has the characteristics of high hardness, uniform thickness, uniform surface color, no ablation, no cracks, no oxidation transition zone, and good corrosion resistance and wear resistance. In addition, the micro-arc oxidation surface treatment through the micro-arc oxidation device with a variable cathode area can simplify the process, and the production rate is controllable and the production cost is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments recorded in the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0030] Figure 1 A schematic structural diagram of a micro-arc oxidation device with a variable cathode area provided in an embodiment of the present application;
[0031] Figure 2 A top view of a micro-arc oxidation tank with a variable cathode area provided in an embodiment of the present application;
[0032] Figure 3 A cross-sectional view of a micro-arc oxidation tank with a variable cathode area provided in an embodiment of the present application;
[0033] Figure 4 A schematic diagram of a micro-arc oxidation surface treatment system with a variable cathode area provided in an embodiment of the present application.
[0034] Figure numerals: 1-micro-arc oxidation tank; 2-circulation tank; 3-lifting mechanism; 4-cooling circulation mechanism; 5-power supply mechanism; 6-workpiece; 7-gantry crane; 8-limiting plate; 9-insulating plate; 11-injection port; 12-outlet; 13-workpiece channel; 14-cathode component; 15-overflow port; 31-curling belt; 32-conductive column; 33-anode component; 34-reduction motor; 81-pressing plate; 82-sealing plate; 83-supporting plate; 91-air distribution hole; 120-liquid level control component; 141-cathode copper bar; 142-stainless steel cathode plate; 10-first cleaning unit; 20-micro-arc oxidation device with variable cathode area; 30-second cleaning unit; 40-drying unit; A-first cleaning tank; B-second cleaning tank; D-third cleaning tank; E-fourth cleaning tank; S-upper hanging area; X-lower hanging area. DETAILED DESCRIPTION
[0035] The present invention is further elaborated below in conjunction with the various embodiments shown in the accompanying drawings, but it should be noted that these embodiments are not limitations of the present invention, and any equivalent transformations or substitutions in functions, methods, or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0036] It should be understood by those skilled in the art that the terms "center", "upper", "lower", "top", "bottom", "inner", "outer", etc. described in this embodiment indicate the orientation or position relationship based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the simplified description of the present invention, rather than indicating or implying that the device or element referred to must be in a specific orientation, constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. The terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features, and in the description of the present invention, unless otherwise specified, "multiple" means two or more. The terms "installation" and "connection" should be understood in a broad sense, for example, it can be either a fixed connection, a detachable connection or an integral connection; it can be either a mechanical connection or an electrical connection; it can be either a direct connection, or an indirect connection through an intermediate medium, or the internal connection of two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the creation of the present invention can be understood by specific circumstances.
[0037] This embodiment provides a micro-arc oxidation device with a variable cathode area. Please refer to Figures 1 to 3 .in, Figure 1 A schematic diagram of the structure of a micro-arc oxidation device with a variable cathode area provided in this embodiment; Figure 2A top view of a micro-arc oxidation tank with a variable cathode area for micro-arc oxidation provided in this embodiment; Figure 3 A cross-sectional view of a micro-arc oxidation tank with a variable cathode area for micro-arc oxidation provided in this embodiment; Figure 4 A schematic diagram of a micro-arc oxidation surface treatment system with a variable cathode area provided in this embodiment.
[0038] Please also see Figures 1 to 3 The micro-arc oxidation device with variable cathode area includes a micro-arc oxidation tank 1, a circulation tank 2, a lifting mechanism 3, a cooling circulation mechanism 4 and a power supply mechanism 5. The micro-arc oxidation tank 1 is provided with an injection port 11, an outflow port 12 and a workpiece channel 13, and a liquid level control member 120 is provided at the end of the outflow port 12. The workpiece channel 13 is located at the bottom of the micro-arc oxidation tank 1, and the width of the workpiece channel 13 is greater than the width of the workpiece 6. A cathode component 14 is provided in the micro-arc oxidation tank 1, and the cathode components 14 are respectively located on both sides of the width direction of the workpiece channel 13, and the cathode component 14 is connected to the negative pole of the power supply mechanism 5. A lifting mechanism 3 is provided above the micro-arc oxidation tank 1, and an anode component 33 is provided on the lifting mechanism 3, and the anode component 33 is connected to the positive pole of the power supply mechanism 5. The lifting mechanism 3 can drive the workpiece 6 to move downward in the micro-arc oxidation tank 1 and pass through the workpiece channel 13. A circulation tank 2 is provided below the micro-arc oxidation tank 1, and a circulation inlet and a circulation outlet are provided on the circulation tank 2. The cooling circulation mechanism 4 connects the outflow port 11 with the circulation inlet and connects the circulation outlet with the injection port 12 , and can cool the electrolyte flowing from the circulation outlet to the injection port 12 .
[0039] The micro-arc oxidation device with variable cathode area provided in the present embodiment is provided with a circulation tank 2 capable of circulating electrolyte below the micro-arc oxidation tank 1, and a liquid level control component 120 and a cooling circulation mechanism 4 are provided at the outflow end of the micro-arc oxidation tank 1, and a lifting mechanism 3 capable of driving the workpiece 6 to move downward at a uniform speed is provided above the micro-arc oxidation tank 1, and a workpiece channel 13 is provided at the bottom of the micro-arc oxidation tank 1, and an anode component 33 connected to the positive electrode of the power supply mechanism 5 is provided on the lifting mechanism 3, and cathode components 14 connected to the negative electrode of the power supply mechanism 5 are provided on both sides of the workpiece channel 13 in the micro-arc oxidation tank 1 in the width direction. The lifting mechanism 3 is turned on to drive the workpiece 6 to immerse in the electrolyte at a uniform speed and then pass through the workpiece channel 13, thereby realizing the zoned micro-arc oxidation of the surface of the workpiece 6. On the one hand, it can be used for micro-arc oxidation surface treatment of large workpieces, and the workpiece does not need to be completely immersed in the electrolyte at one time, thereby improving the growth rate of the micro-arc oxidation film layer, shortening the processing cycle, thereby improving the production efficiency of the micro-arc oxidation film layer, and realizing the recycling of the electrolyte, reducing production energy consumption; on the other hand, the quality of the ceramic film layer can be controlled by controlling the dynamic parameters of the lifting mechanism 3 and the static parameters of the micro-arc oxidation tank 1, so that the ceramic film layer has the characteristics of high hardness, uniform thickness, uniform surface color, no ablation, no cracks, no oxidation transition zone, and good corrosion resistance and wear resistance. In addition, the micro-arc oxidation surface treatment by the micro-arc oxidation device with a variable cathode area can simplify the process, and the production rate is controllable and the production cost is low. Among them, the liquid level control component 120 is a component that can control the liquid level, such as a float valve, various forms of liquid level controllers, etc.
[0040] The cooling circulation mechanism 4 is composed of a pipeline, a valve and a refrigeration mechanism which sequentially connect the micro-arc oxidation tank 1 and the circulation tank 2. The pipeline includes a first pipeline connecting the outflow port 11 and the circulation inlet, and a second pipeline connecting the circulation outlet and the injection port 12. The refrigeration mechanism is arranged in the second pipeline to cool the electrolyte flowing to the injection port 12, so as to realize the circulation refrigeration of the electrolyte.
[0041] The lifting mechanism 3 includes a curling belt 31 and a reduction motor 34. The reduction motor 34 drives the curling belt 31 to perform lifting and lowering movements. A conductive column 32 is horizontally arranged on the curling belt 31, and an anode component 33 is longitudinally arranged on the conductive column 32. A U-shaped clip is provided at one end of the curling belt 31, and the workpiece 6 is fixed to the curling belt 31 through the U-shaped clip. Among them, the anode component 33 is preferably an anode copper bar. When the reduction motor 34 is turned on, the reduction motor 34 drives the curling belt 31 to move downward at a uniform speed, and the workpiece 6 is driven by the curling belt 31 to lift and lower the workpiece 6 at a uniform speed and immerse it in the electrolyte in sections, so as to realize the sectioned continuous scanning oxidation of the workpiece with a large surface area. At the same time, when the workpiece 6 is subjected to sectioned continuous scanning oxidation, the size of the scanning oxidation area is adjusted by adjusting the width of the workpiece channel 13 and adjusting the electrolyte level in the micro-arc oxidation tank 1 by using the liquid level control component 120.
[0042] It should be noted that, in this embodiment, when the micro-arc oxidation groove 1 is installed and connected with the circulation groove 2, the length, width and height of the selected circulation groove 2 are all larger than the micro-arc oxidation groove 1, and each side end of the circulation groove 2 is provided with a channel steel, so that the micro-arc oxidation groove 1 can be set at the notch of the circulation groove 2, making its structure more compact.
[0043] See also Figure 3 As shown, two limit plates 8 are provided at the bottom of the micro-arc oxidation tank 1, and the two limit plates 8 are respectively located on both sides of the width direction of the workpiece channel 13, and each limit plate 8 is provided with a plurality of key grooves in the length direction, so that the width of the workpiece channel 13 can be controlled by adjusting the spacing between the two limit plates 8, which can not only ensure that the workpiece 6 has enough space during the descent process to prevent the workpiece 6 from being scratched and have a positioning function, but also can regulate the flow rate of the electrolyte and adjust the liquid level height, thereby improving the service life and utilization rate of the tank liquid.
[0044] Please continue reading Figure 3 Each limiting plate 8 includes a pressing plate 81, a sealing plate 82 and a supporting plate 83 stacked in sequence from top to bottom, and the width of the sealing plate 82 is greater than the width of the supporting plate 83 and greater than the width of the pressing plate 81, which can not only prevent the workpiece 6 from being scratched by the limiting plate 8 when passing through the workpiece channel 13, but also can position the workpiece 6 so that it can safely pass through the workpiece channel 13. Among them, the sealing plate 82 can be a silicone plate.
[0045] It should be noted that the keyway of each limiting plate 8 can be set at 1 / 4 or 3 / 4 of its length, and each limiting plate 8 can be fixed to the bottom plate of the micro-arc oxidation tank 1 by passing bolts through the keyway.
[0046] In this embodiment, the cathode component 14 includes a cathode copper busbar 141 and a plurality of stainless steel cathode plates 142. The plurality of stainless steel cathode plates 142 are evenly arranged on the inner wall of the micro-arc oxidation tank 1 and are located on both sides of the width direction of the workpiece channel 13. The cathode copper busbar 141 is connected in series with the plurality of stainless steel cathode plates 142, thereby reducing the use of the stainless steel cathode plates 142 while ensuring a smooth and sufficient micro-arc oxidation process, and facilitating the conductive connection between the cathode component 14 and the power supply mechanism 5.
[0047] It should be noted that, in this embodiment, the number of the stainless steel cathode plates 142 is an even number such as 8, 10, 12, etc., and each stainless steel cathode plate 142 is arranged longitudinally on the inner wall of the micro-arc oxidation tank 1, and the cathode copper bar 141 is arranged at the notch of the micro-arc oxidation tank 1 and is laterally connected in series with each stainless steel cathode plate 142. Of course, in order to prevent the cathode copper bar 141 from corroding, the cathode copper bar 141 should always be higher than the liquid level of the electrolyte.
[0048] See also Figure 2An insulating plate 9 is provided at the end of each stainless steel cathode plate 142 which is away from the inner wall of the micro-arc oxidation tank 1. A receiving cavity and a plurality of air distribution holes 91 connected to the receiving cavity are opened in the insulating plate 9. The receiving cavity is connected to an air compression mechanism. The plurality of air distribution holes 91 are located at the end of the insulating plate 9 which is away from the stainless steel cathode plate 142. Thus, the surface of the electrolyte can be kept in a wave-discharging state during the micro-arc oxidation process, thereby ensuring uninterrupted dispersion of the micro-arc oxidation transition zone and eliminating transition color difference.
[0049] See also Figures 2 to 3 The micro-arc oxidation tank 1 is also provided with an overflow port 15, which is located at the notch of the micro-arc oxidation tank 1. When the electrolyte level in the micro-arc oxidation tank 1 is too high, the electrolyte can be discharged into the circulation tank 2 through the overflow port 15, thereby realizing the adjustment of the electrolyte level.
[0050] See also Figure 4 Based on the above research, this embodiment further provides a micro-arc oxidation surface treatment system with a variable cathode area, including the micro-arc oxidation device with a variable cathode area 20, a first cleaning unit 10, a second cleaning unit 30 and a drying unit 40. The first cleaning unit 10, the micro-arc oxidation device with a variable cathode area 20, the second cleaning unit 30 and the drying unit 40 are connected in sequence. Among them, the first cleaning unit 10 includes a first cleaning tank A and a second cleaning tank B; the first cleaning unit 30 includes a third cleaning tank D and a fourth cleaning tank E.
[0051] It should be noted that the micro-arc oxidation surface treatment system with variable cathode area can be controlled and positioned by the gantry crane 7. The specific working process is: the workpiece 6 is hung on the flying bar of the gantry crane 7, and the workpiece 6 is positioned and controlled by the gantry crane, and the workpiece 6 is sequentially cleaned through the first cleaning tank A and the second cleaning tank B, and after removing the dirt and impurities on the surface of the workpiece 6, it enters the micro-arc oxidation device 20 with variable cathode area for segmented scanning oxidation, and then enters the third cleaning tank D and the fourth cleaning tank E in turn for cleaning and impurity removal after oxidation, and enters the drying unit 40 for drying after cleaning, until the lower hanging area, to obtain a ceramic oxide film layer of industrial or building board. In addition, each cleaning tank is equipped with an ultrasonic cleaning unit, and the drying unit 40 is equipped with a heating unit.
[0052] The working process of the micro-arc oxidation surface treatment system with variable cathode area is: the electrolyte is pumped from the circulation tank 2 into the micro-arc oxidation tank 1 through the refrigeration mechanism, and flows into the circulation tank 2 from the outflow port 12 of the oxidation tank 1 and the workpiece channel 13, forming solution circulation refrigeration and utilization. Start the power supply mechanism 5, the ultrasonic cleaning units of each cleaning tank, the heating unit of the drying unit 40, the micro-arc oxidation device with a variable cathode area and other production equipment, drive the gantry crane 7 to the upper hanging area of the conductive column equipped with the plate-type workpiece, and stop it above the micro-arc oxidation tank 1 after primary cleaning and secondary cleaning, start the DC reducer 34 to drive the plate-type workpiece 6 to pass through the workpiece channel 13 to perform a uniform downward motion, and at the same time set the parameters of the power supply mechanism 5 and turn on the power supply mechanism 5 to perform uniform micro-arc oxidation surface treatment. During the micro-arc oxidation surface treatment, the width of the workpiece channel 13 and the height of the float valve at the outflow port 12 are adjusted as needed to realize segmented scanning micro-arc oxidation of the plate-type workpiece 6. After the micro-arc oxidation is completed, it enters the third cleaning tank D and the fourth cleaning tank E in turn for cleaning and impurity removal, and after cleaning, it enters the drying unit 40 for drying until the lower hanging area, to obtain a ceramic oxide film layer for industrial or construction panels.
[0053] Based on the above description, it can be known that the micro-arc oxidation surface treatment system with variable cathode area controls and positions the workpiece 6 through the gantry crane 7, which not only enables the micro-arc oxidation process to be automatically controlled, but also has low equipment requirements and a simple and easy-to-implement process.
[0054] This embodiment also provides a micro-arc oxidation surface treatment method with a variable cathode area, which is implemented by the micro-arc oxidation surface treatment system with a variable cathode area. The surface treatment method specifically includes:
[0055] Cleaning workpieces;
[0056] Using the micro-arc oxidation device with variable cathode area to perform micro-arc oxidation on the cleaned workpiece;
[0057] Cleaning workpieces after micro-arc oxidation;
[0058] Dry the workpiece.
[0059] The micro-arc oxidation surface treatment method with variable cathode area provided in this embodiment, on the one hand, improves the growth rate of the micro-arc oxidation film layer, extends the service life of the workpiece, shortens the processing cycle, and thus improves the production efficiency of the micro-arc oxidation film layer; on the other hand, the process is simple, the production rate is controllable, and the production cost is low. Moreover, the manufactured ceramic film layer has the characteristics of high hardness, uniform thickness, uniform surface color, no ablation, no cracks, no oxidation transition zone, and good corrosion resistance and wear resistance.
[0060] In this embodiment, the electrolyte of the micro-arc oxidation includes 10 g / L sodium silicate, 10 g / L sodium fluoride or potassium fluoride, 10 g / L sodium hydroxide or potassium hydroxide, and the balance water.
[0061] This embodiment also provides the application of the micro-arc oxidation surface treatment method with variable cathode area in manufacturing plate ceramic oxide film layers and alloy plates.
[0062] The implementation scheme of the present application is further described in detail below with reference to specific examples.
[0063] Example 1
[0064] This embodiment 1 provides a method for preparing a ceramic oxide film layer of an industrial or building plate, which specifically includes the following steps:
[0065] Step 1-Prepare raw materials: Select industrial or architectural aluminum alloy plates with dimensions of 2000mm×2000mm×1mm;
[0066] Step 2-Prepare the cleaning mixture: Use metal surface cleaning agent CY-10, add 5% by mass into the cleaning tank 1, turn on gas stirring and ultrasonic cleaning (20-130KHZ);
[0067] Step 3-Preparing a micro-arc oxidation electrolyte: fully stirring 10 g / L of sodium silicate, 10 g / L of sodium fluoride, 10 g / L of sodium hydroxide and water to obtain an electrolyte, and adding the electrolyte into the micro-arc oxidation tank 1;
[0068] Step 4-Set the power supply parameters: voltage 600V, frequency 500HZ, duty cycle 20%; the output pressure of the air compressor is 1-1.2Mpa; the cooling temperature is set to 25-35℃;
[0069] Step 5-micro-arc oxidation: hang the workpiece 6 on the flying bar of the gantry crane 7, and through the positioning and control of the crane, the workpiece is sequentially passed through the first cleaning tank A, the second cleaning tank B, the micro-arc oxidation device with a variable cathode area, the third cleaning tank D, the fourth cleaning tank E, the drying unit 40, until the lower hanging area X, to obtain a ceramic oxide film layer of industrial or building panels, and the height of the electrolyte in the micro-arc oxidation tank is ensured to be 20 cm by adjusting the width of the workpiece channel 13 and the liquid level height of the float valve at the outflow port 12.
[0070] The micro-arc oxidation film layer prepared in this embodiment 1 has uniform color, no transition layer, and an average thickness of the oxidation film layer is 12.3 um, and the surface roughness is 1.17 um.
[0071] Example 2
[0072] This embodiment 2 provides a method for preparing a ceramic oxide film layer of an industrial or building plate, which specifically includes the following steps:
[0073] Step 1-Prepare raw materials: Select industrial or architectural aluminum alloy plates with dimensions of 2000mm×2000mm×1mm;
[0074] Step 2-Prepare the cleaning mixture: Use metal surface cleaning agent CY-10, add 5% by mass into the cleaning tank 1, turn on gas stirring and ultrasonic cleaning (20-130KHZ);
[0075] Step 3-Preparing a micro-arc oxidation electrolyte: fully stirring 10 g / L of sodium silicate, 10 g / L of sodium fluoride, 10 g / L of sodium hydroxide and water to obtain an electrolyte, and adding the electrolyte into the micro-arc oxidation tank 1;
[0076] Step 4-Set the power supply parameters: voltage 620V, frequency 500HZ, duty cycle 22%; the output pressure of the air compressor is 1-1.2Mpa; the cooling temperature is set to 25-35℃;
[0077] Step 5-micro-arc oxidation: hang the workpiece 6 on the flying bar of the gantry crane 7, and through the positioning and control of the crane, the workpiece is sequentially passed through the first cleaning tank A, the second cleaning tank B, the micro-arc oxidation device with a variable cathode area, the third cleaning tank D, the fourth cleaning tank E, the drying unit 40, until the lower hanging area X, to obtain a ceramic oxide film layer of industrial or building panels, and the height of the electrolyte in the micro-arc oxidation tank is ensured to be 20 cm by adjusting the width of the workpiece channel 13 and the liquid level height of the float valve at the outflow port 12.
[0078] The micro-arc oxidation film layer prepared in Example 2 has uniform color, no transition layer, and an average thickness of the oxide film layer of 14.5 um, and a surface roughness of 1.32 um.
[0079] Example 3
[0080] This embodiment 3 provides a method for preparing a ceramic oxide film layer of an industrial or building plate, which specifically includes the following steps:
[0081] Step 1-Prepare raw materials: Select industrial or architectural aluminum alloy plates with dimensions of 2500mm×2500mm×4mm;
[0082] Step 2-Prepare the cleaning mixture: Use metal surface cleaning agent CY-10, add 5% by mass into the cleaning tank 1, turn on gas stirring and ultrasonic cleaning (20-130KHZ);
[0083] Step 3-Preparing a micro-arc oxidation electrolyte: fully stirring 10 g / L of sodium silicate, 10 g / L of sodium fluoride, 10 g / L of sodium hydroxide and water to obtain an electrolyte, and adding the electrolyte into the micro-arc oxidation tank 1;
[0084] Step 4-Set the power supply parameters: voltage 630V, frequency 600HZ, duty cycle 22%; the output pressure of the air compressor is 1-1.2Mpa; the cooling temperature is set to 25-35℃;
[0085] Step 5-micro-arc oxidation: hang the workpiece 6 on the flying bar of the gantry crane 7, and through the positioning and control of the crane, sequentially pass the workpiece through the first cleaning tank A, the second cleaning tank B, the micro-arc oxidation device with a variable cathode area, the third cleaning tank D, the fourth cleaning tank E, the drying unit 40, until the lower hanging area X, to obtain a ceramic oxide film layer of industrial or building panels, and by adjusting the width of the workpiece channel 13 and the liquid level height of the float valve at the outflow port 12, ensure that the height of the electrolyte in the micro-arc oxidation tank is 16 cm.
[0086] The micro-arc oxidation film layer prepared in this embodiment 3 has uniform color, no transition layer, and an average thickness of the oxide film layer is 21.9 um, and the surface roughness is 1.83 um.
[0087] Example 4
[0088] This embodiment 4 provides a method for preparing a ceramic oxide film layer of an industrial or building plate, which specifically includes the following steps:
[0089] Step 1-Prepare raw materials: Select industrial or architectural aluminum alloy plates with dimensions of 2500mm×2500mm×4mm;
[0090] Step 2-Prepare the cleaning mixture: Use metal surface cleaning agent CY-10, add 5% by mass into the cleaning tank 1, turn on gas stirring and ultrasonic cleaning (20-130KHZ);
[0091] Step 3-Preparing a micro-arc oxidation electrolyte: fully stirring 10 g / L of sodium silicate, 10 g / L of sodium fluoride, 10 g / L of sodium hydroxide and water to obtain an electrolyte, and adding the electrolyte into the micro-arc oxidation tank 1;
[0092] Step 4-Set the power supply parameters: voltage 630V, frequency 600HZ, duty cycle 25%; the output pressure of the air compressor is 1-1.2Mpa; the cooling temperature is set to 25-35℃;
[0093] Step 5-micro-arc oxidation: hang the workpiece 6 on the flying bar of the gantry crane 7, and through the positioning and control of the crane, sequentially pass the workpiece through the first cleaning tank A, the second cleaning tank B, the micro-arc oxidation device with a variable cathode area, the third cleaning tank D, the fourth cleaning tank E, the drying unit 40, until the lower hanging area X, to obtain a ceramic oxide film layer of industrial or building panels, and by adjusting the width of the workpiece channel 13 and the liquid level height of the float valve at the outflow port 12, ensure that the height of the electrolyte in the micro-arc oxidation tank is 16 cm.
[0094] The micro-arc oxidation film layer prepared in Example 2 has uniform color, no transition layer, and an average thickness of the oxide film layer is 23.3 um, and a surface roughness of 1.89 um.
[0095] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A micro-arc oxidation device with a variable cathode area, characterized in that: It includes a micro-arc oxidation tank, a circulation tank, a lifting mechanism, a cooling circulation mechanism and a power supply mechanism; The micro-arc oxidation tank is provided with an injection port, an outflow port and a workpiece channel, and a liquid level control component is provided at the outflow port end; the workpiece channel is located at the bottom of the micro-arc oxidation tank, and the width of the workpiece channel is greater than the width of the workpiece; A cathode component is provided in the micro-arc oxidation tank, and the cathode components are respectively located on both sides of the workpiece channel in the width direction, and the cathode components are connected to the negative electrode of the power supply mechanism; The lifting mechanism is provided above the micro-arc oxidation tank, and an anode component is provided on the lifting mechanism, and the anode component is connected to the positive electrode of the power supply mechanism; the lifting mechanism can drive the workpiece to move downward in the micro-arc oxidation tank and pass through the workpiece channel; The circulation groove is provided below the micro-arc oxidation groove, and a circulation inlet and a circulation outlet are provided on the circulation groove. The cooling circulation mechanism connects the outflow port with the circulation inlet, and connects the circulation outlet with the injection port, and can cool the electrolyte flowing from the circulation outlet to the injection port.
2. The micro-arc oxidation device with variable cathode area according to claim 1, characterized in that: Two limit plates are arranged at the bottom of the micro-arc oxidation groove, the two limit plates are respectively located on both sides of the workpiece channel in the width direction, and each limit plate is provided with a plurality of key grooves in the length direction.
3. The micro-arc oxidation device with variable cathode area according to claim 2, characterized in that: Each of the limiting plates comprises a pressing plate, a sealing plate and a supporting plate which are stacked in sequence from top to bottom, and the width of the sealing plate is greater than the width of the supporting plate which is greater than the width of the pressing plate.
4. The micro-arc oxidation device with variable cathode area according to claim 1, characterized in that: The cathode component comprises a plurality of stainless steel cathode plates and cathode copper bars; The plurality of stainless steel cathode plates are evenly arranged on the inner wall of the micro-arc oxidation tank and located on both sides of the width direction of the workpiece channel, and the cathode copper bar connects the plurality of stainless steel cathode plates in series.
5. The micro-arc oxidation device with variable cathode area according to claim 4, characterized in that: An insulating plate is provided at the end of each stainless steel cathode plate which is away from the inner wall of the micro-arc oxidation groove. A accommodating cavity and a plurality of air distribution holes connected to the accommodating cavity are opened in the insulating plate. The accommodating cavity is connected to an air compression mechanism. The plurality of air distribution holes are located at the end of the insulating plate which is away from the stainless steel cathode plate.
6. The micro-arc oxidation device with variable cathode area according to claim 1, characterized in that: An overflow port is also provided on the micro-arc oxidation groove, and the overflow port is located at the groove opening of the micro-arc oxidation groove.
7. A micro-arc oxidation surface treatment system with variable cathode area, characterized in that: A micro-arc oxidation device with a variable cathode area comprising any one of claims 1 to 6, and a first cleaning unit, a second cleaning unit and a drying unit; The first cleaning unit, the micro-arc oxidation device with variable cathode area, the second cleaning unit and the drying unit are connected in sequence.
8. A micro-arc oxidation surface treatment method with a variable cathode area, based on the micro-arc oxidation device with a variable cathode area according to any one of claims 1 to 6, characterized in that: include: Cleaning workpieces; Using the micro-arc oxidation device with variable cathode area to perform micro-arc oxidation on the cleaned workpiece; Cleaning workpieces after micro-arc oxidation; Dry the workpiece.
9. The micro-arc oxidation surface treatment method with variable cathode area according to claim 8, characterized in that: The electrolyte of the micro-arc oxidation includes 10 g / L of sodium silicate, 10 g / L of sodium fluoride or potassium fluoride, 10 g / L of sodium hydroxide or potassium hydroxide and the balance of water.
10. Use of the micro-arc oxidation surface treatment method with variable cathode area according to claim 9 in manufacturing plate ceramic oxide film layers and alloy plates.
Citation Information
Patent Citations
Local electric field controlled microarc oxidation equipment provided with moving cathode
CN101798697A
Anode gradual-entering type microarc oxidation treatment method and device with low energy consumption
CN101845655A