Improvement of blistering and delamination of copper layer in PTH slots of lead-free tin-spraying boards

By adopting graphic electroplating, front baking sheet treatment and post baking sheet treatment in the production of lead-free tin spray PCB boards, the problem of foaming and layering of copper layer is solved, the quality of finished products is improved, and the copper layer and substrate are ensured. Matching avoids quality problems caused by thermal expansion and contraction.

CN114340188BActive Publication Date: 2024-11-19QINGYUAN FUYING ELECTRONICS
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202111651603.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-30
Publication Date
2024-11-19
Estimated Expiration
2041-12-30

AI Technical Summary

Technical Problem

During the production process, the thermal expansion and contraction coefficient of the copper layer is greater than that of the substrate due to high temperature soaking and hot air blowing, resulting in bubbles and delamination of the copper layer in the slot holes, affecting the quality of the finished product.

Method used

Improved production methods are adopted, including graphic plating, front baking sheet treatment, soldering shielding, post baking sheet treatment and tin spraying steps, by performing flattening treatment on the surface of the copper layer, carbon core filtration, impact current process, brightener addition, and electroplating removal The copper layer is stressed, the temperature difference is reduced, the copper layer thickness and thermal expansion and contraction coefficient are controlled to ensure uniformity of the copper layer and matching with the substrate.

Benefits of technology

The foaming and delamination of the copper layer in the slot is effectively avoided, and the quality of the finished product is improved. By increasing the thickness of the copper layer and reducing the temperature difference, the matching between the copper layer and the substrate is ensured, and the quality problems caused by thermal expansion and contraction are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114340188B_ABST
    Figure CN114340188B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lead-free tin-spraying plate, and is particularly a production method for improving the blistering and stratification of the copper layer of the PTH slot of the lead-free tin-spraying plate, including a pre-process, graphic electroplating, outer layer etching, pre-baking plate treatment, solder mask, characters, post-baking plate treatment and post-process steps, wherein: the thickness of the copper layer in the slot of the graphic electroplating is controlled at 25-30um; the pre-baking plate treatment is to bake the plate at 150°C for 45±15 minutes; the post-baking plate treatment is to first perform a normal pre-baking tin treatment on the copper layer of the PTH slot of the lead-free tin-spraying plate, without applying flux, and bake the plate at 150°C for 45±15 minutes. The present invention increases the heat transfer rate due to the increase in the thickness of the copper layer, and the baking plate treatment before solder mask eliminates the stress in the electroplated copper layer. After the baking plate treatment again before tin spraying, the temperature difference during tin spraying is reduced, and the gap between the thermal expansion and contraction coefficient of the copper layer and the substrate is reduced. After the tin spraying treatment, the copper layer in the slot will not produce blistering and stratification, so that the quality of the finished product is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lead-free tin-spraying plates, in particular to a production method for improving blistering and delamination of copper layers in PTH slots of lead-free tin-spraying plates. Background Art

[0002] The PCB board forming process includes the tin spraying process, which is divided into lead tin spraying and lead-free tin spraying. Among them, lead-free tin spraying of PCB boards is environmentally friendly and does not contain harmful substances "lead". The melting point is about 218 degrees. The temperature of the tin spraying furnace needs to be controlled at 280-300 degrees, the peak temperature needs to be controlled at about 260 degrees, and the reflow temperature is 260-270 degrees.

[0003] The existing lead-free tin-spraying PCB production process includes cutting, drilling, PTH slot, copper deposition, full-board electroplating, outer layer circuit, graphic electroplating (electroplated copper layer 20-25um), outer layer etching, solder mask, characters, normal pre-treatment, flux coating, tin-spraying, molding, testing and FQC (final inspection). However, due to the need to be immersed in a high temperature of 270±10℃ for 1-6 seconds during tin-spraying, and 320-420℃, 2-4.5kg / cm 2 The tin surface is leveled by blowing hot air for 2 to 5 seconds. The thermal expansion and contraction coefficient of the copper layer is greater than that of the substrate, which can easily lead to blistering and stratification of the copper layer in the slot after cooling, affecting the quality of the finished product. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] In view of the shortcomings of the prior art, the present invention provides a method for improving the blistering and delamination of the copper layer of the PTH slot of the lead-free tin-spraying board, which solves the problem that the existing lead-free tin-spraying PCB board needs to be immersed in a high temperature of 270±10℃ for 1 to 6 seconds during tin-spraying, and then soaked in a temperature of 320~420℃ and 2~4.5kg / cm 2 The hot air is blown for 2 to 5 seconds to level the tin surface. The thermal expansion and contraction coefficient of the copper layer is greater than that of the substrate, which can easily lead to blistering and stratification of the copper layer in the slot after cooling, affecting the quality of the finished product.

[0006] (II) Technical solution

[0007] In order to achieve the above-mentioned purpose, the present invention specifically adopts the following technical solutions:

[0008] The production method for improving the blistering and delamination of the copper layer of the PTH slot of the lead-free tin-spraying board includes the pre-process, pattern electroplating, outer layer etching, pre-baking board treatment, solder mask, character, post-baking board treatment and post-process steps, wherein:

[0009] In the pattern electroplating process, the surface of the copper layer is flattened and roughened before the pattern electroplating to form a uniform rough surface of 1 to 2 um, so as to increase the contact area with the plating solution and improve the bonding degree with the plating layer; the plating solution is carbon-core filtered before the electroplating to remove organic impurities and oil stains in the plating solution, and the impact current process measures are adopted in the pattern electroplating process to ensure the uniformity of the plating layer in the hole and the consistency of the plating layer thickness, and the brightener is added to the plating solution in an amount of 235 to 260 mL / H.500A (the current is 500A and the brightener is 235 to 260 mL / H) to electroplate a flat and bright copper plating layer, and the thickness of the copper layer in the slot hole is controlled to be within the range of 25 to 30 um;

[0010] In the pre-baking process, the copper-clad laminate after the outer layer etching is baked at 150° C. for 45±15 minutes to remove moisture from the copper-clad laminate and eliminate stress in the electroplated copper layer;

[0011] In the post-baking board treatment, the copper layer of the PTH slot of the copper clad board is first subjected to normal pre-tinning treatment, and the board is baked at 150° C. for 45±15 minutes without applying flux to reduce the temperature difference during tinning and narrow the gap between the thermal expansion and contraction coefficient of the copper layer and the substrate.

[0012] Furthermore, the pre-process steps include cutting, drilling, PTH groove, copper plating, full-board electroplating and outer layer circuit process steps.

[0013] Specifically, after copper is deposited on the copper-clad board, check whether the surface of the copper-plated layer is uniform, smooth the nodules and sand-like blocks on the surface of the copper-plated layer, rinse and dry, and then perform full-board electroplating.

[0014] Furthermore, in the solder resist process, the mesh T number is controlled to be 43T, the squeegee hardness is 65-75 degrees, the ink temperature is controlled at 22-25°C, the ink viscosity is 120-130dps, the developer temperature is 30±2°C, the development time is 60-90 seconds, and the washing pressure is 1.8-2.2kg / cm 2 , the developing point is controlled within 40-60% of the total length of the developing section.

[0015] Furthermore, the post-process steps include applying flux, spraying tin, molding and final inspection process steps.

[0016] Specifically, the lead-free tin-spraying board needs to be immersed in a high temperature of 270±10°C for 1 to 6 seconds, and then 320 to 420°C, 2 to 4.5 kg / cm 2 Blow with hot air for 2 to 5 seconds, and finally level the tin surface.

[0017] (III) Beneficial effects

[0018] Compared with the prior art, the present invention provides a method for improving the blistering and delamination of the copper layer of the PTH slot of the lead-free tin-spraying board, which has the following beneficial effects:

[0019] The invention increases the heat transfer speed due to the increase in the thickness of the copper layer, eliminates the internal stress of the electroplated copper layer by baking the plate before soldering, reduces the temperature difference during tin spraying after baking the plate again before tin spraying, reduces the difference between the thermal expansion and contraction coefficient of the copper layer and the substrate, and then soaks at a high temperature of 270±10°C for 1 to 6 seconds during tin spraying, and is heated at 320 to 420°C and 2 to 4.5kg / cm 2 Hot air is blown for 2 to 5 seconds to level the tin surface. The copper layer in the slot will not bubble or delaminate, which greatly improves the quality of the finished product. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A process flow chart of a method for improving blistering and delamination of copper layers in PTH slots of lead-free tin-spraying boards provided by the present invention. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] like Figure 1 As shown, an embodiment of the present invention provides a method for improving the blistering and delamination of the copper layer of the PTH slot of a lead-free tin-spraying board, including a pre-process, pattern electroplating, outer layer etching, pre-baking board treatment, solder mask, character, post-baking board treatment and post-process steps, wherein:

[0024] In the pattern electroplating process, the surface of the copper layer is flattened and roughened before pattern electroplating to form a uniform rough surface of 2um to increase the contact area with the plating solution and improve the bonding degree with the plating layer; the plating solution is carbon-core filtered before electroplating to remove organic impurities and oil stains in the plating solution. In the pattern electroplating process, impact current process measures are adopted to ensure the uniformity of the plating layer in the hole and the consistency of the plating layer thickness, and brightener is added to the plating solution at a rate of 260mL / H to electroplate a flat and bright copper layer, and the thickness of the copper layer in the slot hole is controlled to be 30um;

[0025] In the pre-baking process, the copper-clad laminate with the outer layer etched is baked at 150°C for 60 minutes to remove moisture from the copper-clad laminate and eliminate stress in the electroplated copper layer.

[0026] In the post-baking board treatment, the copper layer of the PTH slot of the copper clad board is first subjected to normal pre-tinning treatment. Without applying flux, the board is baked at 150°C for 60 minutes to reduce the temperature difference during tinning and narrow the gap between the thermal expansion and contraction coefficient of the copper layer and the substrate.

[0027] In some embodiments, the pre-process steps include cutting, drilling, PTH groove, copper plating, full-board electroplating and outer layer circuit process steps.

[0028] Specifically, after copper is deposited on the copper-clad board, check whether the surface of the copper-plated layer is uniform, smooth the nodules and sand-like blocks on the surface of the copper-plated layer, rinse and dry, and then perform full-board electroplating.

[0029] In some embodiments, in the solder resist process, the mesh T number is controlled to be 43T, the squeegee hardness is 65 degrees, the ink temperature is controlled at 22°C, the ink viscosity is 120dps, the developer temperature is 28°C, the development time is 60 seconds, the water washing pressure is 1.8kg / cm2, and the development point is controlled at 40% of the total length of the development section.

[0030] In some embodiments, the post-process steps include applying flux, spraying tin, molding and final inspection process steps.

[0031] Specifically, the lead-free tin-spraying board needs to be immersed in 280℃ for 6 seconds, and then 420℃, 4.5kg / cm 2 Blow with hot air for 5 seconds and finally level the tin surface.

[0032] Example 2

[0033] like Figure 1 As shown, an embodiment of the present invention provides a method for improving the blistering and delamination of the copper layer of the PTH slot of a lead-free tin-spraying board, including a pre-process, pattern electroplating, outer layer etching, pre-baking board treatment, solder mask, character, post-baking board treatment and post-process steps, wherein:

[0034] In the pattern electroplating process, the surface of the copper layer is flattened and roughened before pattern electroplating to form a uniform rough surface of 1um, so as to increase the contact area with the plating solution and improve the bonding degree with the plating layer; the plating solution is carbon-core filtered before electroplating to remove organic impurities and oil stains in the plating solution. In the pattern electroplating process, impact current process measures are adopted to ensure the uniformity of the plating layer in the hole and the consistency of the plating layer thickness, and brightener is added to the plating solution at a volume of 235mL / H.500A to electroplate a flat and bright copper layer, and the thickness of the copper layer in the slot hole is controlled to be 25um;

[0035] In the pre-baking process, the copper-clad laminate with the outer layer etched is baked at 150°C for 30 minutes to remove moisture from the copper-clad laminate and eliminate stress in the electroplated copper layer.

[0036] In the post-baking board treatment, the copper layer of the PTH slot of the copper clad board is first subjected to normal pre-tinning treatment. Without applying flux, the board is baked at 150°C for 30 minutes to reduce the temperature difference during tinning and narrow the gap between the thermal expansion and contraction coefficient of the copper layer and the substrate.

[0037] In some embodiments, the pre-process steps include cutting, drilling, PTH groove, copper plating, full-board electroplating and outer layer circuit process steps.

[0038] Specifically, after copper is deposited on the copper-clad board, check whether the surface of the copper-plated layer is uniform, smooth the nodules and sand-like blocks on the surface of the copper-plated layer, rinse and dry, and then perform full-board electroplating.

[0039] In some embodiments, in the solder mask process, the mesh T number is controlled to be 43T, the squeegee hardness is 75 degrees, the ink temperature is controlled at 25°C, the ink viscosity is 130dps, the developer temperature is 32°C, the development time is 90 seconds, and the washing pressure is 2.2kg / cm 2 , the developing point is controlled at 60% of the total length of the developing section.

[0040] In some embodiments, the post-process steps include applying flux, spraying tin, molding and final inspection process steps.

[0041] Specifically, the lead-free tin-spraying board needs to be immersed in 260℃ for 2 seconds, and then 320℃, 2kg / cm 2 Blow with hot air for 5 seconds and finally level the tin surface.

[0042] Example 3

[0043] like Figure 1 As shown, an embodiment of the present invention provides a method for improving the blistering and delamination of the copper layer of the PTH slot of a lead-free tin-spraying board, including a pre-process, pattern electroplating, outer layer etching, pre-baking board treatment, solder mask, character, post-baking board treatment and post-process steps, wherein:

[0044] In the graphic electroplating process, the surface of the copper layer is flattened and roughened before the graphic electroplating to form 1.5um to increase the contact area with the plating solution and improve the bonding degree with the plating layer; the plating solution is carbon-core filtered before electroplating to remove organic impurities and oil in the plating solution. In the graphic electroplating process, impact current process measures are adopted to ensure the uniformity of the plating layer in the hole and the consistency of the plating layer thickness, and brightener is added to the plating solution at a volume of 250mL / H.500A to electroplate a flat and bright copper layer, and the thickness of the copper layer in the slot hole is controlled to be 27um;

[0045] In the pre-baking process, the copper-clad laminate with the outer layer etched is baked at 150°C for 45 minutes to remove moisture from the copper-clad laminate and eliminate stress in the electroplated copper layer.

[0046] In the post-baking board treatment, the copper layer of the PTH slot of the copper clad board is first subjected to normal pre-tinning treatment. Without applying flux, the board is baked at 150°C for 45 minutes to reduce the temperature during tinning and reduce the difference between the thermal expansion and contraction coefficient of the copper layer and the substrate.

[0047] In some embodiments, the pre-process steps include cutting, drilling, PTH groove, copper plating, full-board electroplating and outer layer circuit process steps.

[0048] Specifically, after copper is deposited on the copper-clad board, check whether the surface of the copper-plated layer is uniform, smooth the nodules and sand-like blocks on the surface of the copper-plated layer, rinse and dry, and then perform full-board electroplating.

[0049] In some embodiments, in the solder resist process, the mesh T number is controlled to be 43T, the squeegee hardness is 70 degrees, the ink temperature is controlled at 24°C, the ink viscosity is 110dps, the developer temperature is 30°C, the development time is 75 seconds, the water washing pressure is 2kg / cm2, and the development point is controlled at 50% of the total length of the development section.

[0050] In some embodiments, the post-process steps include applying flux, spraying tin, molding and final inspection process steps.

[0051] Specifically, the lead-free tin-spraying board needs to be immersed in 27℃ high temperature for 4 seconds, and then 370℃, 3.2kg / cm 2 Blow with hot air for 4 seconds and finally level the tin surface.

[0052] The lead-free tin-spraying board produced by the production method of Examples 1-3 was inspected for its PTH slot copper layer, and it was found that no bubbles and stratification were generated in the copper layer in the PTH slot. The production method adopted by the present invention increases the heat transfer speed due to the increase in the thickness of the copper layer, and the baking board treatment before soldering eliminates the stress in the electroplated copper layer. After the board is baked again before tin-spraying, the temperature difference during tin-spraying is reduced, and the difference between the thermal expansion and contraction coefficient of the copper layer and the substrate is reduced. Then, the board is immersed in a high temperature of 270±10°C for 1 to 6 seconds during tin-spraying, and is subjected to 320 to 420°C, 2 to 4.5kg / cm 2 Blow hot air for 2 to 5 seconds to level the tin surface, and the copper layer in the slot will not bubble or delaminate.

[0053] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for improving the blistering and delamination of the copper layer of the PTH slot of a lead-free tin-spraying board, characterized in that: It includes pre-process, pattern plating, outer side etching, pre-baking board processing, solder mask, characters, post-baking board processing and post-process steps, among which: In the pattern electroplating process, the surface of the copper layer is flattened and roughened before the pattern electroplating to form a uniform rough surface of 1.5 to 2 um, so as to increase the contact area with the plating solution and improve the bonding degree with the plating layer; the plating solution is carbon-core filtered before electroplating to remove organic impurities and oil stains in the plating solution, and an impact current process measure is adopted during the pattern electroplating process to ensure the uniformity of the plating layer in the hole and the consistency of the plating layer thickness, and a brightener is added to the plating solution at a content of 235 to 260 mL / H to electroplate a flat and bright copper plating layer, and the thickness of the copper layer in the slot hole is controlled to be within the range of 25 to 30 um; In the pre-baking board treatment process, the copper clad board after the outer side etching is baked at 150° C. for 45±15 minutes to remove moisture in the copper clad board and eliminate the internal stress of the electroplated copper layer; In the post-baking board treatment, the copper layer of the PTH slot of the copper clad board is first subjected to normal pre-tinning treatment, and the board is baked at 150° C. for 45±15 minutes without applying flux to reduce the temperature difference during tinning and reduce the difference between the thermal expansion and contraction coefficient of the copper layer and the substrate; In the solder resist process, the mesh T number is controlled to be 43T, the squeegee hardness is 65-75 degrees, the ink temperature is controlled at 22-25°C, the ink viscosity is 120-130dps, the developer temperature is 30±2°C, the development time is 60-90 seconds, and the washing pressure is 1.8-2.2kg / cm 2 , the developing point is controlled within 40-60% of the total length of the developing section, the post-process steps include applying flux, spraying tin, molding and final inspection process steps, the lead-free tin-spraying board needs to be immersed in 270±10℃ for 1-6 seconds, and then 320-420℃, 2-4.5kg / cm 2 Blow with hot air for 2 to 5 seconds, and finally level the tin surface.

2. A method for improving blistering and delamination of copper layer in slots of lead-free tin-spraying boards according to claim 1, characterized in that: The pre-process steps include cutting, drilling, PTH grooving, copper plating, full-board electroplating and outer layer circuit process steps.

3. The method for improving the blistering and delamination of the copper layer of the PTH slot of the lead-free tin-spraying board according to claim 2, characterized in that: After copper is deposited on the copper-clad board, check whether the surface of the copper-plated layer is uniform, smooth the nodules and sand-like blocks on the surface of the copper-plated layer, rinse and dry it, and then electroplate the entire board.

Citation Information

Patent Citations

  • Manufacturing method for heavy-copper printed circuit boards

    CN102821551A

  • Processing method of printed circuit board (PCB) and PCB

    CN103096631A

  • PCB tin spraying and copper removing process

    CN104470223A

  • HASL surface treatment PCB manufacturing method

    CN105376961A

  • LED circuit board solder coating thickness and flatness optimization method

    CN107580424A