A solid oxide fuel cell cathode material with high activity and resistance to Cr poisoning, and its preparation method and application

By attaching PrxFe0.7Co0.3O3 nanoparticles to the surface of the PBSCF cathode, the performance attenuation problem caused by the Cr-containing material in the proton conductor fuel cell is solved, the resistance to Cr poisoning and electrochemical performance is improved, and the service life of the battery is extended.

CN114824315BActive Publication Date: 2024-11-12SOUTH CHINA UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210468923.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-04-29
Publication Date
2024-11-12
Estimated Expiration
2042-04-29

AI Technical Summary

Technical Problem

In proton conductor solid oxide fuel cells, the Cr-containing linker material leads to the problem of attenuation of cathode performance. Existing research focuses less on its Cr poisoning mechanism and anti-Cr poisoning ability under actual operating conditions.

Method used

By attaching PrxFe0.7Co0.3O3 nanoparticles to the cathode surface of PrBa0.5Sr0.5Co1.5Fe0.5O5+ (PBSCF), the impregnation method is used to improve the redox reaction activity and anti-Cr poisoning ability.

Benefits of technology

It significantly improves the ORR activity and anti-Cr poisoning ability of the PBSCF cathode, extends the service life of the battery, and shows higher electrochemical performance and durability under actual PCFCs operating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114824315B_ABST
    Figure CN114824315B_ABST
Patent Text Reader

Abstract

The present invention discloses a solid oxide fuel cell cathode material with high activity and Cr poisoning resistance, as well as a preparation method and application thereof. In order to solve the problem of rapid attenuation of battery cathode performance caused by volatile Cr generated by stainless steel connector materials in the service environment of proton conductor solid oxide fuel cells PCFCs, an impregnation method was successfully used to prepare a PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& (PBSCF) A large amount of Pr x Fe 0.7 Co 0.3 O3 (PFC) nanoparticles greatly improve the ORR activity and Cr poisoning resistance of the PBSCF cathode. The method has the characteristics of simple process, low cost, and easy operation. The present invention has theoretical and practical significance for promoting the development of long-life cathode materials for PCFCs (with high ORR activity, high water resistance and Cr poisoning resistance).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of high-temperature fuel cells, and in particular relates to a solid oxide fuel cell cathode material with high activity and resistance to Cr poisoning, and a preparation method and application thereof. Background Art

[0002] Solid oxide fuel cells are a promising technology that can efficiently generate electricity from a variety of fuels and can alleviate the growing global energy demand, characterized by high energy conversion efficiency, low emissions, and good fuel flexibility. Ba-based cathode materials, such as the ion-ordered double perovskite structure PrBa 0.8 Ca 0.2 Co2O 5+& (PBCC) and PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& (PBSCF) materials, compared with single perovskite structure materials at medium and low temperatures (500-700℃), have easier oxygen ion diffusion, faster surface oxygen exchange and higher ion conductivity, and have been widely studied as cathode materials for proton conductor solid oxide fuel cells (PCFCs). However, when using Cr-containing connector materials, such as SUS430 and Crofer22APU, high-valent volatile substances (such as CrO3 and CrO2[OH]2) will be generated under high temperature, oxidizing atmosphere and certain humidity. They diffuse through the gas to the entire cathode and the three-phase interface, react with Sr or Ba segregated in the cathode material to form low-conductivity phase SrCrO4, BaCrO4 and BaCr2O4 deposited on the cathode surface, resulting in a decrease in the cathode's oxidation ability, causing cathode performance degradation, and then causing the battery's electrochemical performance to decay. This phenomenon is called cathode Cr poisoning. Unlike oxygen ion conductor solid oxide fuel cells (O-SOFCs), water vapor is generated on the cathode side of the cell in PCFCs, and its presence will aggravate the segregation of Sr or Ba in the cathode, while intensifying the generation and diffusion of volatile Cr species, thereby accelerating Cr poisoning at the cathode.

[0003] However, few studies have focused on the Cr poisoning mechanism of the cathode under actual PCFCs operating conditions when Cr-containing interconnects are used, and on the electrochemical performance, Cr poisoning resistance, and long-term stability of the single cells composed of them. Therefore, when Cr-containing interconnects are used, long-life cathode materials suitable for PCFCs (with high ORR activity, high water resistance, and Cr poisoning resistance) are still urgently needed.

[0004] Jin Li et al. developed a La2NiO 4+δ Attached PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+δ Cathode materials, study the anti-Cr effect of LNO-PBSCF in oxygen ion conductor solid oxide fuel cells. In the study by Jin Li et al., the long-term stability of the battery when LNO-PBSCF was used as the cathode of proton conductor solid oxide fuel cells, water was passed through the cathode, and Cr-containing interconnects were used (J.Li, J.Li, D.Yan, J.Pu, B.Chi, L.Jian, Promoted Cr-poisoning tolerance of La2NiO 4+δ -coated PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+δ cathode for intermediate temperature solid oxide fuel cells, Electrochim. Acta, 270 (2018) 294-301.). Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a solid oxide fuel cell cathode material with high activity and resistance to Cr poisoning, as well as a preparation method and application thereof. In order to solve the problem of battery cathode performance degradation caused by volatile Cr generated by stainless steel interconnect materials in the service environment of proton conductor solid oxide fuel cells PCFCs, an impregnation method was successfully used to prepare a PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& (PBSCF) A large amount of Pr x Fe 0.7 Co 0.3 O3 (PFC) nanoparticles greatly improve the ORR (redox reaction) activity and Cr poisoning resistance of the PBSCF cathode. The method has the characteristics of simple process, low cost, and easy operation. The present invention has theoretical and practical significance for promoting the development of long-life cathode materials for PCFCs (with high ORR activity, high water resistance and Cr poisoning resistance).

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] The present invention provides a solid oxide fuel cell cathode material with high activity and Cr poisoning resistance, wherein the solid oxide fuel cell cathode material with high activity and Cr poisoning resistance is composed of Pr x Fe 0.7 Co 0.3 O3(PFC)-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& (PBSCF), where 0.8≤x≤1, & represents the oxygen vacancy content.

[0008] Furthermore, Pr x Fe 0.7 Co 0.3 O3 nanoparticles are uniformly attached to the PBSCF main phase.

[0009] Furthermore, the nanoparticle phase Pr x Fe 0.7 Co 0.3 The main elements of O3 are: Pr, Co, Fe and O, and the particle size of PFC nanoparticles is 20nm.

[0010] Furthermore, the main elements of the PBSCF main phase are: Pr element, Ba element, Sr element, Co element, Fe element and O element, and the particle size of the PBSCF main phase is 100-300nm.

[0011] The present invention provides a method for preparing a solid oxide fuel cell cathode material with high activity and Cr poisoning resistance, comprising the following steps:

[0012] (1) Pr(NO3)3·6H2O, Ba(NO3)2, Sr(NO3)2, Co(NO3)2·6H2O, and Fe(NO3)3·9H2O are added into water to dissolve and heated and stirred to be uniform; glycine and citric acid monohydrate are added to evaporate the water under heating and stirring conditions to obtain a gel-like substance; the gel-like substance is placed in a drying process to obtain a PBSCF cathode material precursor, and the PBSCF cathode material precursor is then calcined to obtain a PBSCF cathode material powder;

[0013] (2) Pr(NO3)3·6H2O, Co(NO3)2·6H2O and Fe(NO3)3·9H2O were dissolved in water to obtain Pr x Fe 0.7 Co 0.3 O3 precursor solution, to Pr x Fe 0.7 Co 0.3Surfactants and complexing agents are added to the O3 precursor solution to obtain Pr x Fe 0.7 Co 0.3 O3 catalyst solution;

[0014] (3) Pr x Fe 0.7 Co 0.3 The O3 catalyst solution was impregnated on the surface of the PBSCF cathode material, calcined, and the impregnation and calcination process was repeated to obtain Pr x Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& , recorded as PFC-PBSCF cathode material.

[0015] Furthermore, in step (1), the molar ratio of glycine to citric acid monohydrate is 1:(0.5-2); 3+ , Ba 2+ , Sr 2+ 、Co 2+ , Fe 3+ The molar ratio of total metal ions: glycine: citric acid monohydrate is 1: (0.5-1): (0.5-1).

[0016] Furthermore, in step (1), the molar ratio of glycine to citric acid monohydrate is one of (1:0.5), (0.5:1), (0.75:0.75), (0.75:1), and (1:0.75).

[0017] Further, in step (1), Pr 3+ , Ba 2+ , Sr 2+ 、Co 2+ , Fe 3+ The molar ratio of total metal ions: glycine: citric acid monohydrate is 1:0.75:0.75.

[0018] Furthermore, the molar ratio of glycine to citric acid monohydrate is (0.5-1):(0.5-1).

[0019] Further, the molar ratio of glycine to citric acid monohydrate is 1:1.

[0020] Furthermore, the drying process in step (1) is carried out at 250-300° C. for 2-5 hours.

[0021] Furthermore, the calcination conditions in step (1) are 900-950° C. for 2-4 hours.

[0022] Furthermore, in step (2), the molar ratio of Pr(NO3)3·6H2O to Co(NO3)2·6H2O is (0.8-1):0.3; the molar ratio of Pr(NO3)3·6H2O to Fe(NO3)3·9H2O is (0.8-1):0.7.

[0023] Furthermore, the surfactant in step (2) is polyvinyl pyrrolidone; the mass ratio of the total mass of Pr(NO3)3·6H2O, Co(NO3)2·6H2O, and Fe(NO3)3·9H2O in step (2) to the surfactant is 1:5%.

[0024] Furthermore, the complexing agent in step (2) is glycine; and the molar ratio of the total number of moles of NO3- in Pr(NO3)3·6H2O, Co(NO3)2·6H2O, and Fe(NO3)3·9H2O to the complexing agent in step (2) is 2:1.

[0025] Furthermore, in step (3), the calcination temperature is 700-800°C; the calcination time is 1-3h; the heating and cooling rates during the calcination process are both 3-5°C / min; and the number of repetitions is 1-3 times.

[0026] Furthermore, the preparation method of the main phase PBSCF cathode material comprises the following steps:

[0027] The preparation method of PBSCF cathode powder is prepared by sol-gel method.

[0028] Furthermore, the sol-gel method comprises the following steps:

[0029] According to the stoichiometric ratio, Pr(NO3)3·6H2O, Ba(NO3)2, Sr(NO3)2, Co(NO3)2·6H2O and Fe(NO3)3·9H2O are sequentially added into deionized water to dissolve and heat and stir evenly; glycine and citric acid monohydrate are added, and the water is evaporated under heating and stirring to obtain a gel-like substance; the gel-like substance is placed in an oven for drying to obtain a PBSCF cathode material precursor, and the PBSCF cathode material precursor is then placed in a muffle furnace for roasting to obtain a PBSCF cathode material powder.

[0030] Further, the preparation method of PFC-PBSCF cathode material

[0031] The PFC-PBSCF cathode material was synthesized by impregnation method. Stoichiometric high-purity Pr(NO3)3·6H2O, Co(NO3)2·6H2O and Fe(NO3)3·9H2O were dissolved in deionized water to prepare 0.1 M Pr x Fe 0.7 Co 0.3 O3 (PFC) precursor solution. A surfactant, polyvinylpyrrolidone (PVP) (5 wt%), was added to the 0.1 M solution to improve the wetting / permeability of the solution, thereby ensuring uniform dispersion of the impregnated material. A certain amount of glycine was added as a complexing agent. Then 5 μL of Pr x Fe 0.7 Co 0.3 The O3(PFC) catalyst solution was impregnated on the porous PBSCF cathode surface. Under the capillary force, the solution was absorbed into the pores of the skeleton. Then it was calcined at 700℃ for 1h. The heating / cooling rate was 5℃min -1 The catalyst loading was measured after heat treatment and increased by repeating the infiltration process.

[0032] The present invention also provides application of the PFC-PBSCF cathode material prepared by the preparation method in a fuel cell.

[0033] Furthermore, the fuel cell is a proton conductor solid oxide fuel cell.

[0034] Furthermore, PFC-PBSCF is used in proton conductor solid oxide fuel cells (PCFCs). Under actual PCFCs operating conditions, when Cr-containing interconnects are used, PFC-PBSCF simultaneously has high ORR activity, high resistance to water and Cr poisoning.

[0035] Furthermore, the proton conductor solid oxide fuel cell (PCFCs) is configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF.

[0036] Further, the proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF has a structure including a proton conductor electrolyte BZCYYb, and a Ni-BZCYYb anode and a PFC-PBSCF cathode located on both sides of the proton conductor electrolyte;

[0037] Furthermore, the Ni-BZCYYb anode refers to Ni-BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-& (Ni-BZCYYb) anode.

[0038] Furthermore, the chemical formula of the proton conductor electrolyte BZCYYb is BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-& .

[0039] Furthermore, the method for preparing the proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF is to first prepare a Ni-BZCYYb anode support half-cell (including a BZCYYb electrolyte layer, a Ni-BZCYYb anode support layer and a Ni-BZCYYb anode functional layer) by co-casting and co-sintering. The PBSCF cathode slurry is screen-printed on the electrolyte surface of the half-cell, and then placed in a high-temperature muffle furnace and calcined at 950° C. for 2 hours to obtain the desired Ni-BZCYYb|BZCYYb|PBSCF single cell. Then, the PFC catalyst is impregnated on the PBSCF cathode surface by an impregnation method to obtain a Ni-BZCYYb|BZCYYb|PFC-PBSCF single cell.

[0040] Furthermore, the co-casting and co-sintering method of the Ni-BZCYYb anode support half-cell is as follows: First, the electrolyte slurry, the anode functional layer slurry and the anode support slurry are sequentially cast on the polymer film, and then dried in the air for 12 hours; after it is dried, a 15 cm diameter grinder is used to knock it into about 100 small pieces, and then the pieces are placed in a high-temperature muffle furnace and calcined at 600 ° C for 2 hours (this process is the degreasing process). During the degreasing process, a slow heating rate is used to remove the organic components in the sheet. Finally, the degreased sheet is placed in a high-temperature muffle furnace and calcined at 1450 ° C for 5 hours to obtain the desired Ni-BZCYYb anode support half-cell.

[0041] Furthermore, the Ni-BZCYYb anode consists of two layers: an anode functional layer (20 μm thick) and an anode support layer (800 μm thick). The anode functional layer has finer pores and a larger surface area, providing more three-phase boundaries for electrochemical reactions. The anode support layer has larger pores and continuous channels, providing a convenient path for gas transport.

[0042] Furthermore, the preparation method of PBSCF cathode slurry is as follows: weigh 1 g PBSCF cathode powder, 0.004 g PVB (polyvinyl butyral), and 0.076 g pineol, pour them into a mortar and grind them for 1-3 hours to obtain the desired PBSCF cathode slurry.

[0043] Furthermore, the effective area of ​​the PBSCF cathode slurry by screen printing is 0.2826 cm2 .

[0044] Furthermore, the preparation method of BZCYYb powder is to adopt a solid phase method.

[0045] Furthermore, the solid phase method comprises the following steps: dissolving high-purity barium carbonate, zirconium oxide, cerium oxide, ytterbium oxide and yttrium oxide powders in ethanol according to a stoichiometric ratio and ball milling for 24 hours to mix evenly, placing the mixed solution in an oven to dry to obtain a dry powder, and then pressing the dry powder into tablets, placing it in a muffle furnace and calcining it at 1100°C for 12 hours. Then, the calcined powder is added to ethanol and high-energy ball milled again for 4 hours, pressed into tablets after drying, and then placed in a muffle furnace and calcined at 1100°C for 12 hours to obtain a pure perovskite phase. After adding the obtained powder to ethanol and high-energy ball milling for 4 hours, the desired BZCYYb powder is obtained.

[0046] Furthermore, the tableting is performed at a pressure of 10 MPa.

[0047] Furthermore, the current collection method of the proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF is to connect the electrode surface with silver wires for current collection using silver paste (DAD-87, purchased from Shanghai Synthetic Resin Research Institute).

[0048] Beneficial Effects

[0049] 1. The PFC-PBSCF cathode material involved in the present invention is a material that successfully attaches a large amount of Pr on the surface of the PBSCF cathode by using an impregnation method. x Fe 0.7 Co 0.3 O3(PFC) nanoparticles greatly improve the ORR activity and anti-Cr poisoning ability of the PBSCF cathode. 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-& The electrochemical performance and durability of the single cell supported by the (Ni-BZCYYb) anode are also significantly enhanced in the presence of a Cr source (Crofer22APU). In addition, Raman analysis shows that the PFC catalyst can prevent the PBSCF cathode surface from being directly exposed to the Cr source, thereby alleviating the accumulation of the BaCrO4 insulating phase on the PBSCF cathode.

[0050] 2. The preparation method of the present invention has the characteristics of simple process, low cost, easy operation, etc. The present invention has theoretical and practical significance for promoting the development of long-life cathode materials for PCFCs (having high ORR activity, high water resistance and resistance to Cr poisoning). BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 The Pr in the PFC-PBSCF cathode material prepared in Example 1 of the present invention 0.9 Fe 0.7 Co 0.3 XRD pattern of O3 catalyst phase.

[0052] Figure 2 The PFC-PBSCF cathode material prepared in Example 1 of the present invention is attached with Pr 0.9 Fe 0.7 Co 0.3 XRD pattern of PBSCF of O3 nanoparticle phase.

[0053] Figure 3a This is the SEM image of PBSCF impregnated with PFC nanoparticles in Example 1.

[0054] Figure 3b This is a HR-TEM (high resolution transmission electron microscope) image of the PFC-PBSCF cathode material prepared in Example 1 of the present invention.

[0055] Figure 4a This is a SEM image of each layer of the proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF involved in the present invention.

[0056] Figure 4b PrBa of Application Example 1 of the present invention 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& (PBSCF) SEM image of the cathode layer.

[0057] Figure 4c For BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 SEM image of O3(BZCYYb).

[0058] Figure 5 The present invention relates to a configuration of PBSCF|BZCYYb|PBSCF and a configuration of P x FC-PBSCF|BZCYYb|P x FC-PBSCF (x = 0.8, 0.9 and 1) (P x A comparison chart of polarization resistance of a symmetrical battery with an FC impregnation volume of 5 μL and a test temperature of 550-700°C, with dry air passing through the cathode and no Cr sheet placed.

[0059] Figure 6The configuration involved in the present invention is P 0.9 FC-PBSCF|BZCYYb|P 0.9 A comparison chart of the polarization resistance of a symmetrical battery of FC-PBSCF at different impregnation amounts when the test temperature is 550-700℃, dry air is passed through the cathode, and no Cr sheet is placed.

[0060] Figure 7 The long-term stability comparison diagram of polarization resistance of symmetrical batteries configured as PBSCF|BZCYYb|PBSCF and configured as PFC-PBSCF|BZCYYb|PFC-PBSCF involved in the present invention is shown at a test temperature of 650°C, with dry air / humidified air passing through the cathode and with and without a Cr sheet placed.

[0061] Figure 8 The present invention provides a comparison of IVP curves of the proton conductor solid oxide fuel cells configured as Ni-BZCYYb|BZCYYb|PBSCF and Ni-BZCYYb|BZCYYb|PFC-PBSCF tested in the range of 550-700°C when using hydrogen as fuel gas for power generation.

[0062] Fig. 9 The present invention relates to a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF and configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF, when generating electricity using hydrogen as fuel gas, at a test temperature of 650°C, with dry air / humidified air passing through the cathode, and with and without a Cr sheet placed. The present invention relates to a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF, when generating electricity using hydrogen as fuel gas, and at a test temperature of 650°C.

[0063] Fig.10 The present invention relates to a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF and configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF. When generating electricity using hydrogen as fuel gas, the test temperature is 650°C, humidified air is passed through the cathode, and a Cr sheet is placed under the test conditions. After a long-term test of a single cell for 100 hours, the Raman characterization diagram of the surface of the PBSCF cathode and the PFC-PBSCF cathode is shown. DETAILED DESCRIPTION

[0064] The present invention is further described in detail below in conjunction with examples and drawings, but the embodiments of the present invention are not limited thereto.

[0065] The anode material and proton conductor solid oxide fuel cell involved in the present invention include but are not limited to the materials in the following embodiments, and the optimization method and preparation method involved include but are not limited to the methods in the following embodiments. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the invention shall be included in the protection scope of the present invention.

[0066] Example 1

[0067] This embodiment provides a Pr 0.9 Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& The preparation method of cathode material, the specific steps are as follows:

[0068] (1) 8.696 g Pr(NO3)3·6H2O, 2.614 g Ba(NO3)2, 2.116 g Sr(NO3)2, 8.731 g Co(NO3)2·6H2O, and 4.04 g Fe(NO3)3·9H2O were added to 100 ml deionized water to dissolve and heated at 130° C. and stirred uniformly; 4.504 g glycine and 12.608 g citric acid monohydrate were added, and the water was evaporated under the condition of heating and stirring at 130° C. for 5 h to obtain a gel-like substance; the gel-like substance was placed in a 300° C. oven for 2 h to dry to obtain a PBSCF cathode material precursor, and the PBSCF cathode material precursor was then calcined at 900° C. for 2 h to obtain a PBSCF cathode material powder;

[0069] (2) Dissolve 0.392 g Pr(NO3)3·6H2O, 0.087 g Co(NO3)2·6H2O and 0.283 g Fe(NO3)3·9H2O in 10 ml water to obtain Pr 0.9 Fe 0.7 Co 0.3 O3 precursor solution, to Pr 0.9 Fe 0.7 Co 0.3 0.038 g of surfactant polyvinylpyrrolidone PVP and 0.203 g of glycine complexing agent were added to the O3 precursor solution to obtain a Pr 0.9 Fe 0.7 Co 0.3 O3 catalyst solution;

[0070] (3) Add 2.5 μL of 0.1 mol / L Pr 0.9 Fe 0.7 Co0.3 The O3 catalyst solution was impregnated on the surface of the PBSCF cathode material and covered the entire cathode surface. Under the capillary force, the solution was absorbed into the pores of the PBSCF skeleton to obtain an impregnated sample. The impregnated sample was then placed in a muffle furnace and calcined in an air atmosphere at 700°C for 3h with a heating / cooling rate of 5°C min -1 The impregnation and calcination process was repeated to obtain a loading of 0.205 mg cm -2 Pr 0.9 Fe 0.7 Co 0.3 O3 catalyst Pr 0.9 Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& , recorded as PFC-PBSCF cathode material.

[0071] Application Example 1

[0072] This application example specifically provides a method of 0.9 Symmetrical battery with FC-PBSCF as cathode material (configured as P 0.9 FC-PBSCF|BZCYYb|P 0.9 The polarization resistance test of FC-PBSCF) at 550°C to 700°C in moist air (≈3% H2O) with a Cr source includes the following specific steps:

[0073] (1) Take 1 g of the PBSCF cathode material powder prepared in Example 1, 0.004 g of PVB, and 0.076 g of pinene alcohol, pour them into a mortar and grind them for 2 h to obtain the required PBSCF cathode slurry.

[0074] (2) The obtained PBSCF cathode slurry was screen-printed on the surface of the dense electrolyte BZCYYb, and then calcined in a high-temperature muffle furnace at 950°C for 2 h to obtain the desired PBSCF|BZCYYb|PBSCF symmetric battery (the area of ​​the PBSCF cathode layer screen-printed was 0.2826 cm 2 ).

[0075] (3) Then, using a microinjector, 2.5 μL of the P prepared in Example 1 was added. 0.9 The FC catalyst impregnation liquid was impregnated on the cathode surface of PBSCF, dried at 70℃, and then 2.5μLP 0.9The FC catalyst impregnation solution was continuously impregnated on the PBSCF cathode surface to obtain an impregnated sample, which was then fired in an air atmosphere at 700 °C for 3 h with a heating / cooling rate of 5 °C min -1 , and get P 0.9 The FC catalyst loading was 0.41 mg cm -2 P 0.9 FC-PBSCF|BZCYYb|P 0.9 FC-PBSCF single cell.

[0076] (4) The polarization resistance was then tested using an electrochemical workstation (AMETEK PARSTAT MC) at 550°C to 700°C in the presence of a Cr source in humid air (≈3% H2O).

[0077] The preparation method of BZCYYb powder is to adopt a solid phase method.

[0078] 54.644g high-purity barium carbonate (purity 99.99%), 3.42g zirconium oxide (purity 99.99%), 33.361g cerium oxide (purity 99.99%), 5.456g ytterbium oxide (purity 99.99%) and 3.12g yttrium oxide (purity 99.99%) powders were dissolved in ethanol, ball milled for 24 hours to mix evenly, and the mixed solution was placed in an oven to dry to obtain a dry powder, and then the dry powder was pressed into a sheet with a pressure of 10Mpa, and placed in a muffle furnace for calcination at 1100°C for 12 hours. Then the calcined powder was added to ethanol and ball milled again at high energy (500r / min) for 4 hours, and after drying, it was pressed into a sheet with a pressure of 10Mpa, and then placed in a muffle furnace for calcination at 1100°C for 12 hours to obtain a pure perovskite phase. The obtained powder was added into ethanol and ball-milled at high energy (500 r / min) for 4 h to obtain the desired BZCYYb powder.

[0079] Preparation of proton conductor solid oxide fuel cells configured as Ni-BZCYYb|BZCYYb|PBSCF and proton conductor solid oxide fuel cells configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF

[0080] (1) Preparation of BZCYYb slurry: 6 g BZCYYb, 0.2 g fish oil dispersant, and 3 g anhydrous ethanol were mixed evenly to obtain BZCYYb slurry. Preparation of anode functional layer slurry: 2.4 g BZCYYb, 3.6 g nano-NiO, 0.6 g graphite pore former, 0.2 g fish oil dispersant, and 3 g anhydrous ethanol were mixed evenly to obtain anode functional layer slurry. Preparation of anode support slurry: 20 g BZCYYb, 30 g NiO, 3 g graphite pore former, 2 g fish oil dispersant, and 12 g anhydrous ethanol were mixed evenly to obtain anode support slurry.

[0081] (1) 9.2 g of BZCYYb slurry, 9.8 g of anode functional layer slurry and 67 g of anode support slurry were sequentially cast on a PET (polyethylene terephthalate) release film polymer film, and then dried in air for 12 h; after drying, a 15 cm diameter grinder was used to knock it into 100 small pieces (with a diameter of 15 cm), and then the pieces were placed in a high-temperature muffle furnace and calcined at 600 ° C for 2 h (this process is the degreasing process). During the degreasing process, a slow heating rate (1 ° C / min) was used to remove the organic components in the piece. Finally, the degreased sheet was placed in a high-temperature muffle furnace and calcined at 1450°C for 5 hours to obtain the required Ni-BZCYYb anode support half-cell, which included a BZCYYb electrolyte layer, a Ni-BZCYYb anode support layer (800 μm thick) and a Ni-BZCYYb anode functional layer (20 μm thick).

[0082] (2) The PBSCF cathode slurry prepared from the PBSCF cathode material powder prepared in Example 1 was screen-printed on the electrolyte surface of the half-cell, and then placed in a high-temperature muffle furnace and calcined at 950° C. for 2 h to obtain the desired Ni-BZCYYb|BZCYYb|PBSCF proton conductor solid oxide fuel cell. Then, the PFC catalyst was impregnated on the PBSCF cathode surface by an impregnation method to obtain a Ni-BZCYYb|BZCYYb|PFC-PBSCF proton conductor solid oxide fuel cell.

[0083] Application Example 2

[0084] This application example 2 specifically provides a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF and a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF when using a Cr-containing connector material, and the output power test specifically includes the following specific steps:

[0085] (1) Before the electrochemical test, the electrode surface was partially connected to the silver mesh using silver paste (DAD-87, purchased from Shanghai Synthetic Resin Research Institute) for current collection.

[0086] (2) Use ceramic sealant to seal the battery.

[0087] (3) Place a Cr sheet (Crofer22APU) on the cathode.

[0088] (4) A proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF and a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF were heated to 700°C in ambient air.

[0089] (5) Pass nitrogen gas (flow rate: 20 ml / min) for 5 min to exhaust all air in the tube.

[0090] (6) After the air in the tube is purged, the nitrogen is cut into humidified H2 (the volume percentage of water in H2 is 3%) (flow rate is 30 ml / min) for reducing the anode, and the cathode is exposed to the ambient air.

[0091] (7) When H2 is passed into the anode for 20 min, the battery is observed to have a stable OCV (open circuit voltage).

[0092] (8) The open circuit voltage (OCV), current-voltage (IV), and impedance spectrum characteristics of the battery in a hydrogen atmosphere were tested using an electrochemical workstation (AMETEK PARSTAT MC) at a test temperature of 550°C to 700°C.

[0093] Example 2

[0094] This embodiment provides a Pr 0.8 Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& The preparation method of cathode material, the specific steps are as follows:

[0095] (1) 8.696 g Pr(NO3)3·6H2O, 2.614 g Ba(NO3)2, 2.116 g Sr(NO3)2, 8.731 g Co(NO3)2·6H2O, and 4.04 g Fe(NO3)3·9H2O were added to 100 ml deionized water to dissolve and heated at 130° C. and stirred to be uniform; 6.006 g glycine and 8.405 g citric acid monohydrate were added, and the water was evaporated under the condition of heating and stirring at 130° C. for 5 h to obtain a gel-like substance; the gel-like substance was placed in an oven at 275° C. for 3 h to dry to obtain a PBSCF cathode material precursor, and the PBSCF cathode material precursor was then calcined at 900° C. for 4 h to obtain a PBSCF cathode material powder;

[0096] (2) Dissolve 0.348 g Pr(NO3)3·6H2O, 0.087 g Co(NO3)2·6H2O and 0.283 g Fe(NO3)3·9H2O in 10 ml water to obtain Pr 0.8 Fe 0.7 Co 0.3 O3 precursor solution, to Pr 0.8 Fe 0.7 Co 0.3 0.036 g of surfactant polyvinylpyrrolidone PVP and 0.191 g of glycine complexing agent were added to the O3 precursor solution to obtain a Pr 0.8 Fe 0.7 Co 0.3 O3 catalyst solution;

[0097] (3) Add 2.5 μL of 0.1 mol / L Pr 0.9 Fe 0.7 Co 0.3 The O3 catalyst solution was impregnated on the surface of the PBSCF cathode material and covered the entire cathode surface. Under the capillary force, the solution was absorbed into the pores of the PBSCF skeleton to obtain an impregnated sample. The impregnated sample was then placed in a muffle furnace and calcined in an air atmosphere at 800°C for 1 h, with a heating / cooling rate of 3°C min -1 The impregnation and calcination steps were repeated twice to obtain a loading of 0.41 mg cm -2 Pr 0.8 Fe 0.7 Co 0.3 O3 catalyst Pr 0.8 Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& , denoted as P0.8 FC-PBSCF cathode material.

[0098] Example 3

[0099] This embodiment provides a P1rFe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& The preparation method of cathode material, the specific steps are as follows:

[0100] (1) 8.696 g Pr(NO3)3·6H2O, 2.614 g Ba(NO3)2, 2.116 g Sr(NO3)2, 8.731 g Co(NO3)2·6H2O, and 4.04 g Fe(NO3)3·9H2O were dissolved in 100 ml deionized water and heated at 130°C and stirred to be uniform; 3.003 g glycine and 16.811 g citric acid monohydrate were added, and the water was evaporated under the condition of heating and stirring at 130°C for 5 h to obtain a gel-like substance; the gel-like substance was placed in an oven at 250°C for 5 h to dry to obtain a PBSCF cathode material precursor, and the PBSCF cathode material precursor was then calcined at 950°C for 3 h to obtain a PBSCF cathode material powder;

[0101] (2) Dissolve 0.435 g Pr(NO3)3·6H2O, 0.087 g Co(NO3)2·6H2O and 0.283 g Fe(NO3)3·9H2O in 10 ml water to obtain Pr1Fe 0.7 Co 0.3 O3 precursor solution, to Pr1Fe 0.7 Co 0.3 0.04 g of surfactant polyvinylpyrrolidone PVP and 0.214 g of glycine complexing agent were added to the O3 precursor solution to obtain a Pr1Fe 0.7 Co 0.3 O3 catalyst solution;

[0102] (3) Add 2.5 μL of 0.1 mol / L Pr1Fe 0.7 Co 0.3 The O3 catalyst solution was impregnated on the surface of the PBSCF cathode material and covered the entire cathode surface. Under the capillary force, the solution was absorbed into the pores of the PBSCF skeleton to obtain an impregnated sample. The impregnated sample was then placed in a muffle furnace and calcined in an air atmosphere at 750°C for 2h with a heating / cooling rate of 4°C min -1 The impregnation and calcination process was repeated three times to obtain a loading of 0.615 mg cm-2 Pr1Fe 0.7 Co 0.3 O3 catalyst Pr1Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& , recorded as PFC-PBSCF cathode material.

[0103] Characterization results

[0104] 1. XRD characterization

[0105] Figure 1 Pr prepared in Example 1 of the present invention 0.9 Fe 0.7 Co 0.3 The XRD pattern of O3 catalyst phase is shown in Figure 2. Figure 1 It can be seen that Pr 0.9 Fe 0.7 Co 0.3 The lattice parameter of the O3 catalyst phase is close to that of La 0.6 Sr 0.4 Co 0.8 Fe 0.2 O3, indicating that the PFC catalyst is in a single perovskite phase; Figure 2 The PFC-PBSCF cathode material prepared in Example 1 of the present invention is attached with Pr 0.9 Fe 0.7 Co 0.3 XRD pattern of PBSCF of O3 nanoparticle phase, which is double perovskite phase.

[0106] 2. Electron microscopy characterization

[0107] Figure 3a The SEM image of PBSCF impregnated with PFC nanoparticles in Example 1 is shown in FIG. Figure 3a It can be seen that the PFC nanoparticle phase with a particle size of 20 nm is attached to the PBSCF main phase with a particle size of 100-300 nm. Figure 3b HR-TEM image of the PFC-PBSCF cathode material prepared in Example 1 of the present invention, Figure 3b It can also be seen that the PFC nanoparticle phase with a diameter of 20nm is attached to the PBSCF main phase with a particle size of 100-300nm.

[0108] Scanning electron microscope (SEM) images of the layers of a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF are presented in Figure 4a In, from Figure 4aIt can be seen that the battery has four layers: a porous anode support layer (ASL, Ni-BZCYYb, 800 μm thick), an anode functional layer (AFL, Ni-BZCYYb, 20 μm thick), a dense electrolyte (BZCYYb, 7 μm thick) and a porous cathode (PBSCF, 50 μm thick). The PBSCF cathode layer was obtained by applying step (2) of Example 1. Figure 4b PrBa of Application Example 1 of the present invention 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& SEM image of the cathode layer of (PBSCF), Figure 4b It can be seen that the cathode has a porous structure, which is convenient for air transmission. Figure 4c For BaZr 0.1 Ce 0.7 Y 0.1 Yb 0.1 O 3-& SEM image of (BZCYYb), Figure 4c It can be seen that the electrolyte layer has been sintered densely.

[0109] 3. Characterization of polarization resistance of cathode materials

[0110] Figure 5 The present invention relates to a configuration of PBSCF|BZCYYb|PBSCF and a configuration of P x FC-PBSCF|BZCYYb|P x FC-PBSCF (x = 0.8, 0.9 and 1) (P x The comparison of polarization resistance of the symmetrical battery with FC impregnation volume of 5μL at 550℃, 600℃, 650℃, and 700℃, with dry air passing through the cathode and no Cr sheet placed, is shown in the figure. Figure 5 It can be seen that P 0.9 The FC-PBSCF cathode has the smallest polarization resistance value.

[0111] Figure 6 The configuration involved in the present invention is P 0.9 FC-PBSCF|BZCYYb|P 0.9 Symmetrical cells of FC-PBSCF were tested at 550℃, 600℃, 650℃, and 700℃, with dry air flowing through the cathode and no Cr sheet placed, and different impregnation amounts (P 0.9 The impregnation amount of FC was 0.205 mg cm -2 , 0.41 mg cm -2 , 0.615 mg cm -2 ) when the polarization resistance is compared, it can be seen that Figure 6 When the impregnation volume is 5 μL (i.e. 0.41 mg cm -2 ), the cathode has the smallest polarization resistance value.

[0112] Figure 7 The present invention relates to a configuration of PBSCF|BZCYYb|PBSCF and a configuration of P 0.9 FC-PBSCF|BZCYYb|P 0.9 Symmetrical cell of FC-PBSCF, tested at 650℃, with dry air / humidified air (≈3% H2O) flowing through the cathode, with and without Cr sheet, the long-term stability comparison of polarization resistance shows that the PFC-PBSCF cathode shows a smaller R than the blank PBSCF cathode under all conditions. p The values ​​and decay rates indicate that the PFC-PBSCF cathode material has enhanced ORR activity and significantly improved resistance to Cr poisoning.

[0113] 4. Output power characterization

[0114] Figure 8 The present invention provides a comparison of IVP curves of a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF and a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF tested in the range of 550-700°C when generating electricity using hydrogen as fuel gas. It can be seen that the single cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF exhibits a higher peak power density than the Ni-BZCYYb|BZCYYb|PBSCF single cell under different operating conditions (temperature 500-700°C, with / without Cr source, dry air / humid air (≈3% H2O). For example, at 650°C, the peak power density of the single cell of the catalyst impregnated Ni-BZCYYb|BZCYYb|PFC-PBSCF in the presence of Cr pollution and dry air is 1.15 W cm -2 , is a single cell with blank cathode Ni-BZCYYb|BZCYYb|PBSCF performance (0.786W cm -2 ) is nearly 1.5 times.

[0115] 5. Single cell stability characterization

[0116] Fig. 9The proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF and the proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF of the present invention generate electricity using hydrogen as fuel gas. Under the test conditions of a test temperature of 650°C, dry air / humidified air (≈3% H2O) passing through the cathode, and with and without a Cr sheet, the constant current density is 0.5Acm -2 From the relationship between the voltage and time of a single cell, it can be seen that the decay rate of the Ni-BZCYYb|BZCYYb|PFC-PBSCF single cell impregnated with catalyst is significantly reduced.

[0117] Fig.10 The present invention relates to a proton conductor solid oxide fuel cell configured as Ni-BZCYYb|BZCYYb|PBSCF and configured as Ni-BZCYYb|BZCYYb|PFC-PBSCF. When generating electricity using hydrogen as fuel gas, the test temperature is 650°C, humidified air (≈3% H2O) is passed through the cathode, and a Cr sheet is placed. After a single cell is subjected to a long-term test for 100 hours, the Raman characterization diagram of the surface of the PBSCF cathode and the PFC-PBSCF cathode is shown. Figure 8 It can be seen that Raman analysis shows that the PFC catalyst can prevent the PBSCF cathode surface from being directly exposed to the Cr source, thereby alleviating the accumulation of BaCrO4 insulating phase on the PBSCF cathode.

Claims

1. A method for preparing a solid oxide fuel cell cathode material with high activity and resistance to Cr poisoning, characterized in that: The following steps are involved: (1) Pr(NO3)3·6H2O, Ba(NO3)2, Sr(NO3)2, Co(NO3)2·6H2O, and Fe(NO3)3·9H2O are added into water to dissolve and heated and stirred to be uniform; glycine and citric acid monohydrate are added, and water is evaporated under heating and stirring to obtain a gel-like substance; Drying the gel-like substance to obtain a PBSCF cathode material precursor, and then calcining the PBSCF cathode material precursor to obtain a PBSCF cathode material powder; (2) Dissolve Pr(NO3)3·6H2O, Co(NO3)2·6H2O and Fe(NO3)3·9H2O in water to obtain Pr x Fe 0.7 Co 0.3 O3 precursor solution, to Pr x Fe 0.7 Co 0.3 Surfactants and complexing agents are added to the O3 precursor solution to obtain Pr x Fe 0.7 Co 0.3 O3 catalyst solution; (3) Pr x Fe 0.7 Co 0.3 The O3 catalyst solution was impregnated on the surface of the PBSCF cathode material, calcined, and the impregnation and calcination process was repeated to obtain Pr x Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& , denoted as PFC-PBSCF cathode material, wherein 0.8≤x≤1, & represents the oxygen vacancy content; the calcination temperature is 700-800°C; and the calcination time is 1-3h.

2. The method for preparing a solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning according to claim 1, characterized in that: In step (1), the molar ratio of glycine to citric acid monohydrate is 1:(0.5-2); Pr 3+ , Ba 2+ , Sr 2+ 、Co 2+ , Fe 3+ The molar ratio of total metal ions: glycine: citric acid monohydrate is 1:(0.5-1):(0.5-1).

3. The method for preparing a solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning according to claim 1, characterized in that: In step (1), the drying temperature is 250-300°C, and the drying time is 2-5 hours; the roasting temperature is 900-950°C, and the roasting time is 2-4 hours.

4. The method for preparing a solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning according to claim 1, characterized in that: In step (2), the molar ratio of Pr(NO3)3·6H2O to Co(NO3)2·6H2O is (0.8-1):0.3; the molar ratio of Pr(NO3)3·6H2O to Fe(NO3)3·9H2O is (0.8-1):0.

7.

5. The method for preparing a solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning according to claim 1, characterized in that: The surfactant in step (2) is polyvinyl pyrrolidone (PVP).

6. The method for preparing a solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning according to claim 1, characterized in that: The complexing agent in step (2) is glycine.

7. The method for preparing a solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning according to claim 1, characterized in that: In step (3), the heating and cooling rates during the calcination process are both 3-5°C / min; the number of repetitions is 1-3 times.

8. A solid oxide fuel cell cathode material having high activity and resistance to Cr poisoning obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The solid oxide fuel cell cathode material with high activity and resistance to Cr poisoning is composed of Pr x Fe 0.7 Co 0.3 O3-PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& , Pr x Fe 0.7 Co 0.3 O3 is recorded as PFC, PrBa 0.5 Sr 0.5 Co 1.5 Fe 0.5 O 5+& Denoted as PBSCF.

9. Use of the PFC-PBSCF cathode material prepared by the preparation method according to any one of claims 1 to 7 in a fuel cell.

10. The use of the PFC-PBSCF cathode material in a fuel cell according to claim 9, characterized in that: The fuel cell is a proton conductor solid oxide fuel cell.