A sodium ion lithium battery electrode material and preparation method thereof
Through the combination of modified graphene and composite electrode materials, a sodium-ion lithium battery electrode material with high discharge specific capacity and long cycle stability is prepared, which solves the problem of rapid capacity fading of electrode materials in the existing technology and achieves The effect of 99% capacity retention after 1000 cycles.
Patent Information
- Application Number
- CN202210857471.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-07-20
AI Technical Summary
Existing lithium battery electrode materials have problems such as rapid capacity fading and unstable cycle performance during long-term cycle use, and cannot meet market demand.
Using a combination of modified graphene, composite electrode materials and stabilizers, nanoparticles are prepared through hydrothermal reaction and high-temperature calcination methods to form layered structures and flower-like structures, which enhance the electrochemical reaction area and conductivity, and are coated with carbon Form an electronic conductive network.
The sodium-ion lithium battery electrode material has achieved high discharge specific capacity and excellent long-term cycle stability. The capacity retention rate is more than 99% after 1000 cycles, which has broad application prospects.
Smart Images

Figure BDA0003756146770000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a sodium ion lithium battery electrode material and a preparation method thereof. Background Art
[0002] Since the 21st century, energy issues have become the main problem restricting the economic development of various countries. Traditional fossil energy such as coal, oil and natural gas is currently the main energy source supporting social development. However, not only is the problem of fossil energy reserves becoming increasingly prominent, but it also brings serious environmental pollution. Therefore, the development of clean renewable energy has become the key to the sustainable development of human society. In the current energy storage system, chemical energy storage batteries stand out due to their high efficiency, convenience, and no geographical restrictions, and have become a hot topic of research worldwide.
[0003] Compared with fuel power systems, lithium batteries are widely used due to their zero-emission advantage. With the improvement of public environmental awareness, the demand for lithium battery energy storage devices is increasing. HEV, PEV and other vehicles equipped with power lithium batteries have developed rapidly, and the demand for lithium battery electrode materials has also grown explosively. Sodium-ion batteries have abundant sodium sources, which can be extracted from seawater and salt lakes, providing possibilities for the sustainable development of batteries. In recent years, people's research on lithium batteries has mainly focused on how to improve the mass capacity, volume capacity, charge and discharge efficiency, cycle performance and other factors of lithium batteries. The most common and effective approach is to modify the negative and positive electrode materials. For example, Chinese patent CN2020010478674 discloses a method for preparing a lithium battery electrode material based on graphene modification, which comprises modifying the lithium battery negative electrode material and graphene, and coating the modified graphene on the surface of the lithium battery electrode material to form a coating layer, thereby reducing the contact area between the lithium battery negative electrode material and the battery electrolyte, and improving the cycle performance and charge and discharge performance of the lithium battery. Although this technical solution can effectively improve the charge and discharge performance of the lithium battery, it cannot effectively slow down the attenuation rate of the electrode material capacity, resulting in the long cycle performance of the lithium battery being not stable enough, and there are certain limitations in use, which cannot meet market demand well. Summary of the invention
[0004] The object of the present invention is to provide a sodium ion lithium battery electrode material and a preparation method thereof, which not only has a high discharge specific capacity and can meet normal practical needs, but also has excellent long-cycle stability. After 1,000 cycles, the capacity retention rate is above 99%, and the material has extremely broad application prospects.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A sodium ion lithium battery electrode material and a preparation method thereof, comprising the following raw materials in parts by weight: 1-5 parts of modified graphene, 0.1-0.5 parts of a dispersant, 0.1-0.5 parts of a stabilizer, 3-8 parts of an active substance, 20-30 parts of a composite electrode material, and 60-80 parts of deionized water.
[0007] As a preferred technical solution of the present invention, the dispersant is selected from at least one of hydroxymethyl cellulose, hydroxyethyl cellulose and ethyl cellulose;
[0008] The stabilizer is selected from at least one of fatty acid zinc, hydrotalcite, and diisooctyl phosphite;
[0009] The active substance is selected from at least one of hydroxybenzenesulfonic acid, hydroxybenzenesulfonate, and benzenesulfonic acid.
[0010] As a preferred technical solution of the present invention, the preparation method of the modified graphene is as follows:
[0011] 1) adding cobalt acetate tetrahydrate, nickel acetate tetrahydrate and polyvinyl pyrrolidone to ethylene glycol, stirring at 400-600 r / min for 30-60 min, then adding graphene, and continuing stirring for 20-50 min to obtain a precursor solution;
[0012] 2) The precursor solution is transferred to a hydrothermal reactor, and heat-insulated in a hydrothermal oven. After cooling to room temperature, the precipitated precursor is poured into an ethanol solution, ultrasonically shaken at 200-400W for 10-30min, centrifuged and repeatedly washed with deionized water, and the product is frozen and vacuum freeze-dried at -50--60°C using a freeze dryer, and then transferred to a muffle furnace for heat-insulation treatment, and naturally cooled to room temperature to obtain modified graphene.
[0013] As a preferred technical solution of the present invention, the usage ratio of cobalt acetate tetrahydrate, nickel acetate tetrahydrate, polyvinyl pyrrolidone, ethylene glycol and graphene is (1-5) g: (0.5-2.5) g: (0.025-0.045) g: (40-60) mL: (5-15) mL.
[0014] As a preferred technical solution of the present invention, the holding temperature in the hydrothermal oven is 180-190°C, and the holding time is 12-15h;
[0015] The insulation temperature in the muffle furnace is 380-420° C., and the insulation time is 2-5 hours.
[0016] As a preferred technical solution of the present invention, the preparation method of the composite electrode material is as follows:
[0017] 1) dissolving tetrabutyl titanate in an ethanol solution, stirring magnetically for 10-30 min to prepare solution A, then mixing aluminum nitrate nonahydrate, ammonium dihydrogen phosphate and lithium acetate dihydrate, grinding them into a paste, and then adding them to solution A, stirring magnetically at 60-70° C. for 1-3 h, transferring to a muffle furnace for heating treatment, cooling to room temperature, and ball milling to obtain nanoparticles for standby use;
[0018] 2) nickel nitrate hexahydrate and cobalt nitrate hexahydrate are placed in a container, ethanol solution is added, and magnetic stirring is performed at room temperature for 30-50 minutes to obtain a precursor solution, and an ammonia solution is added dropwise to the precursor solution, titrated to a pH of 7.5-8.5, and then allowed to stand for 10-15 hours, the product is repeatedly washed with distilled water and ethanol, filtered, placed in a constant temperature drying oven at 80-90° C. and dried for 20-25 hours, and ground to obtain a composite nanomaterial;
[0019] 3) The nanoparticles are mixed with the composite nanomaterial to form mixed particles, which are then evenly mixed with sucrose and added to an acetone solution. The mixed solution is stirred magnetically to be evenly dispersed until the acetone is completely volatilized, and then the temperature is raised to 600-650°C at 2-5°C / min, kept in an argon environment for 3-6 hours, and naturally cooled to room temperature to obtain a composite electrode material.
[0020] As a preferred technical solution of the present invention, the ratio of tetrabutyl titanate, ethanol, aluminum nitrate nonahydrate, ammonium dihydrogen phosphate, and lithium acetate dihydrate is (11.5-15.5) g: (500-800) mL: (2.2-3.0) g: (6.9-8.2) g: (2.9-3.6) g;
[0021] The muffle furnace heating treatment parameters are as follows: first heat at 450-500°C for 2-5h, then heat to 800-860°C and keep warm for 3-6h.
[0022] As a preferred technical solution of the present invention, the ratio of the nickel nitrate hexahydrate to the cobalt nitrate hexahydrate and the ethanol solution is (5-10) mmol: (2.5-5.0) mmol: (25-50) mL;
[0023] The concentration of the ammonia solution is 0.6-0.8 mol / L.
[0024] As a preferred technical solution of the present invention, the mass ratio of the nanoparticles to the composite nanomaterial is 5:1-3;
[0025] The sucrose accounts for 10-30% of the total mass of the mixed particles.
[0026] A method for preparing a sodium ion lithium battery electrode material, the specific preparation method comprising the following steps:
[0027] According to the weight fraction, the modified graphene, dispersant, stabilizer, active substance and deionized water are stirred and dispersed for 1-5 hours to obtain a dispersion, the dispersion is homogenized at a pressure of 100-400 MPa for 1-5 times, the composite electrode material is added, stirred at a speed of 1000-6000 rpm for 1-5 hours, and after drying, heat-treated at 200-400° C. for 2-6 hours in a nitrogen atmosphere, crushed and sieved to obtain a lithium battery electrode material.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] In the present invention, tetrabutyl titanate, aluminum nitrate nonahydrate, ammonium dihydrogen phosphate and lithium acetate dihydrate are used as raw materials, a precursor is prepared by a sol-gel method, and a high-temperature calcination method is used to make the raw material particles contact each other, and the atoms diffuse in the solid phase, and a new phase nucleates and grows at the contact interface, so as to obtain nanoparticles with a high sodium ion diffusion coefficient. The nanoparticles are small in size, have a large electrochemical reaction area and a short sodium ion migration distance, and show an excellent sodium ion diffusion coefficient, which is conducive to releasing the internal stress generated when embedding / de-embedding sodium ions, improving the stability of the SEI film structure on the surface of the material, and thus helping to improve the long-cycle stability of the electrode material; at the same time, the nanoparticles are used Nickel nitrate hexahydrate and cobalt nitrate hexahydrate are used as raw materials to prepare a layered composite nanomaterial through a chemical coprecipitation method. The layered structure of the composite nanomaterial is composed of a large number of nanosheets that cross each other. The interconnected nanosheet structures can effectively increase the electrochemical reaction specific surface area of the electrode and promote the contact between the electrode interface and the electrolyte solution. At the same time, the edges of the nanosheets can also create more electrochemical active sites for the electrochemical reaction, thereby improving the electrochemical performance of the electrode. By mixing the above two and then carbon-coating them, the conductivity of the carbon layer is utilized to form an electronic conductive network on the surface, so that the composite electrode material has excellent conductivity and excellent cycle stability.
[0030] In the present invention, graphene is used as a matrix, cobalt acetate tetrahydrate and nickel acetate tetrahydrate are used as raw materials, and a flower-like structure composed of a large number of two-dimensional thin sheets is deposited on the surface of the graphene. Each flower-like structure is interconnected and can play a supporting role, thereby avoiding structural collapse caused by volume expansion, thereby preventing the SEI film on the surface of the material from being damaged, thereby reducing side reactions with the electrolyte, thereby slowing down the attenuation rate of the capacity of the electrode material, and achieving further enhancement of the cycle stability of the electrode material.
[0031] The lithium battery electrode material provided in the present invention not only has a high discharge specific capacity and can meet normal practical needs, but also has excellent long-cycle stability. After 1,000 cycles, the capacity retention rate is above 99%, and has extremely broad application prospects. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Example 1
[0034] A sodium ion lithium battery electrode material and a preparation method thereof, comprising the following raw materials in parts by weight: 1 part of modified graphene, 0.1 part of a dispersant, 0.1 part of a stabilizer, 3 parts of an active substance, 20 parts of a composite electrode material, and 60-80 parts of deionized water;
[0035] Among them, the dispersant is hydroxymethyl cellulose;
[0036] The stabilizer is fatty acid zinc;
[0037] The active substance is hydroxybenzenesulfonic acid.
[0038] Wherein, the preparation method of modified graphene is as follows:
[0039] 1) Add 1 g of cobalt acetate tetrahydrate, 0.5 g of nickel acetate tetrahydrate and 0.025 g of polyvinyl pyrrolidone to 40 mL of ethylene glycol, stir at 400 r / min for 30 min, then add 5 g of graphene, and continue stirring for 20 min to obtain a precursor solution;
[0040] 2) The precursor solution is transferred to a hydrothermal reactor, kept at 180°C in a hydrothermal oven for 12 hours, cooled to room temperature, poured into an ethanol solution, ultrasonically shaken at 200W for 10 minutes, centrifuged and repeatedly washed with deionized water, and the product is frozen and vacuum freeze-dried at -50°C using a freeze dryer, then transferred to a muffle furnace, kept at 380°C for 2 hours, and naturally cooled to room temperature to obtain modified graphene.
[0041] The preparation method of the composite electrode material is as follows:
[0042] 1) Dissolve 11.5 g of tetrabutyl titanate in 500 mL of ethanol solution, stir magnetically for 10 min to prepare solution A, then weigh 2.2 g of aluminum nitrate nonahydrate, 6.9 g of ammonium dihydrogen phosphate and 2.9 g of lithium acetate dihydrate, mix and grind into a paste, then add to solution A, stir magnetically for 1 h at 60 ° C, transfer to a muffle furnace, heat at 450 ° C for 2 h, then heat to 800 ° C for 3 h, cool to room temperature, and obtain nanoparticles after ball milling for standby use;
[0043] 2) Weigh 5 mmol of nickel nitrate hexahydrate and 2.5 mmol of cobalt nitrate hexahydrate into a container, add 25 mL of ethanol solution, and stir magnetically at room temperature for 30 min to obtain a precursor solution. Add 0.6 mol / L ammonia solution dropwise into the precursor solution, titrate to a pH of 7.5, and then let stand for 10 h. Wash the product repeatedly with distilled water and ethanol, filter it, put it in a constant temperature drying oven at 80° C. and dry it for 20 h. Grind it to obtain a composite nanomaterial;
[0044] 3) The above nanoparticles and composite nanomaterials are mixed in a mass ratio of 5:1 to form mixed particles, which are then evenly mixed with sucrose and added to an acetone solution, with the sucrose accounting for 10% of the total mass of the mixed particles. The mixed solution is stirred magnetically to be evenly dispersed until the acetone is completely volatilized, and then heated to 600°C at 2°C / min, kept warm for 3 hours in an argon environment, and naturally cooled to room temperature to obtain an electrode material.
[0045] A method for preparing a sodium ion lithium battery electrode material, the specific preparation method comprising the following steps:
[0046] According to the weight fraction, the modified graphene, dispersant, stabilizer, active substance and deionized water are stirred and dispersed for 1 hour to obtain a dispersion, the dispersion is homogenized once at a pressure of 100 MPa, the composite electrode material is added, and the mixture is stirred at a speed of 1000 rpm for 1 hour. After drying, the mixture is heat treated at 200°C for 2 hours in a nitrogen atmosphere, and the powder is crushed and sieved to obtain the lithium battery electrode material.
[0047] Example 2
[0048] A sodium ion lithium battery electrode material and a preparation method thereof, comprising the following raw materials in parts by weight: 3 parts of modified graphene, 0.3 parts of a dispersant, 0.3 parts of a stabilizer, 5 parts of an active substance, 25 parts of a composite electrode material, and 70 parts of deionized water;
[0049] Among them, hydroxyethyl cellulose is selected as the dispersant;
[0050] The stabilizer is hydrotalcite;
[0051] The active substance is benzenesulfonic acid.
[0052] Wherein, the preparation method of modified graphene is as follows:
[0053] 1) Add 3 g of cobalt acetate tetrahydrate, 1.5 g of nickel acetate tetrahydrate and 0.035 g of polyvinyl pyrrolidone to 50 mL of ethylene glycol, stir at 500 r / min for 50 min, then add 10 g of graphene, and continue stirring for 35 min to obtain a precursor solution;
[0054] 2) The precursor solution is transferred to a hydrothermal reactor, kept at 185°C in a hydrothermal oven for 13 hours, cooled to room temperature, poured into an ethanol solution, ultrasonically shaken at 300W for 20 minutes, centrifuged and repeatedly washed with deionized water, and the product is frozen and vacuum freeze-dried at -55°C using a freeze dryer, then transferred to a muffle furnace, kept at 400°C for 3 hours, and naturally cooled to room temperature to obtain modified graphene.
[0055] The preparation method of the composite electrode material is as follows:
[0056] 1) Dissolve 13.5 g of tetrabutyl titanate in 650 mL of ethanol solution, stir magnetically for 20 min to prepare solution A, then weigh 2.8 g of aluminum nitrate nonahydrate, 7.3 g of ammonium dihydrogen phosphate and 3.2 g of lithium acetate dihydrate, mix and grind into a paste, then add to solution A, stir magnetically at 65° C. for 2 h, transfer to a muffle furnace, heat at 480° C. for 3 h, then heat to 840° C. for 5 h, cool to room temperature, and obtain nanoparticles after ball milling for standby use;
[0057] 2) Weigh 8 mmol of nickel nitrate hexahydrate and 3.5 mmol of cobalt nitrate hexahydrate into a container, add 40 mL of ethanol solution, and stir magnetically at room temperature for 40 min to obtain a precursor solution. Add 0.7 mol / L ammonia solution dropwise into the precursor solution, titrate to pH 8.0, and then let stand for 13 h. Wash the product repeatedly with distilled water and ethanol, filter it, put it in a constant temperature drying oven at 85°C and dry it for 23 h. Grind it to obtain a composite nanomaterial;
[0058] 3) The above nanoparticles and the composite nanomaterials are mixed in a mass ratio of 5:2 to form mixed particles, which are then evenly mixed with sucrose and added to an acetone solution, with the sucrose accounting for 20% of the total mass of the mixed particles. The mixed solution is stirred magnetically to be evenly dispersed until the acetone is completely volatilized, and then the temperature is raised to 620°C at 3°C / min, kept in an argon environment for 5 hours, and naturally cooled to room temperature to obtain an electrode material.
[0059] A method for preparing a sodium ion lithium battery electrode material, the specific preparation method comprising the following steps:
[0060] According to the weight fraction, the modified graphene, dispersant, stabilizer, active substance and deionized water are stirred and dispersed for 3 hours to obtain a dispersion, the dispersion is homogenized twice under a pressure of 200 MPa, the composite electrode material is added, stirred at a speed of 5000 rpm for 2 hours, and after drying, heat treated at 300°C for 5 hours in a nitrogen atmosphere, and crushed and sieved to obtain the lithium battery electrode material.
[0061] Example 3
[0062] A sodium ion lithium battery electrode material and a preparation method thereof, comprising the following raw materials in parts by weight: 5 parts of modified graphene, 0.5 parts of a dispersant, 0.5 parts of a stabilizer, 8 parts of an active substance, 30 parts of a composite electrode material, and 80 parts of deionized water;
[0063] Among them, the dispersant is ethyl cellulose;
[0064] The stabilizer is diisooctyl phosphite;
[0065] The active substance is benzenesulfonic acid.
[0066] Wherein, the preparation method of modified graphene is as follows:
[0067] 1) 5 g of cobalt acetate tetrahydrate, 2.5 g of nickel acetate tetrahydrate and 0.045 g of polyvinyl pyrrolidone were added to 60 mL of ethylene glycol, stirred at 600 r / min for 60 min, and then 15 g of graphene was added, and stirring was continued for 50 min to obtain a precursor solution;
[0068] 2) The precursor solution is transferred to a hydrothermal reactor, kept at 190°C in a hydrothermal oven for 15 hours, cooled to room temperature, poured into an ethanol solution, ultrasonically shaken at 400W for 30 minutes, centrifuged and repeatedly washed with deionized water, and the product is frozen and vacuum freeze-dried at -60°C using a freeze dryer, then transferred to a muffle furnace, kept at 420°C for 5 hours, and naturally cooled to room temperature to obtain modified graphene.
[0069] The preparation method of the composite electrode material is as follows:
[0070] 1) Dissolve 15.5 g of tetrabutyl titanate in 800 mL of ethanol solution, stir magnetically for 30 min to prepare solution A, then weigh 3.0 g of aluminum nitrate nonahydrate, 8.2 g of ammonium dihydrogen phosphate and 3.6 g of lithium acetate dihydrate, mix and grind into a paste, then add to solution A, stir magnetically for 3 h at 70 ° C, transfer to a muffle furnace, heat at 500 ° C for 5 h, then heat to 860 ° C for 6 h, cool to room temperature, and obtain nanoparticles after ball milling for standby use;
[0071] 2) Weigh 10 mmol of nickel nitrate hexahydrate and 5.0 mmol of cobalt nitrate hexahydrate into a container, add 50 mL of ethanol solution, and stir magnetically at room temperature for 50 min to obtain a precursor solution. Add 0.8 mol / L ammonia solution dropwise into the precursor solution, titrate to a pH of 8.5, and then let stand for 15 h. Wash the product repeatedly with distilled water and ethanol, filter it, put it in a 90°C constant temperature drying oven and dry it for 25 h, and grind it to obtain a composite nanomaterial;
[0072] 3) The above nanoparticles and composite nanomaterials are mixed in a mass ratio of 5:3 to form mixed particles, which are then evenly mixed with sucrose and added to an acetone solution, wherein the sucrose accounts for 30% of the total mass of the mixed particles. The mixed solution is stirred magnetically to be evenly dispersed until the acetone is completely volatilized, and then the temperature is raised to 650°C at 5°C / min, kept in an argon environment for 6 hours, and naturally cooled to room temperature to obtain an electrode material.
[0073] A method for preparing a sodium ion lithium battery electrode material, the specific preparation method comprising the following steps:
[0074] According to the weight fraction, the modified graphene, dispersant, stabilizer, active substance and deionized water are stirred and dispersed for 5 hours to obtain a dispersion, the dispersion is homogenized at a pressure of 400 MPa for 5 times, the composite electrode material is added, stirred at a speed of 6000 rpm for 5 hours, and after drying, heat treated at 400°C for 6 hours in a nitrogen atmosphere, and crushed and sieved to obtain the lithium battery electrode material.
[0075] Comparative Example 1: This comparative example is substantially the same as Example 1, except that graphene is used instead of modified graphene.
[0076] Comparative Example 2: This comparative example is basically the same as Example 1, except that step 2) in the electrode material preparation method is omitted.
[0077] Comparative Example 3: This comparative example is basically the same as Example 1, except that step 2) in the electrode material preparation method is omitted, and graphene is used instead of modified graphene.
[0078] The electrode materials provided in Examples 1-3 and Comparative Examples 1-3 were selected as samples, 80% of the sample, 15% of acetylene carbon black and 5% of polyvinylidene fluoride were mixed and evenly coated on a stainless steel mesh as a working electrode, a platinum wire was used as a counter electrode, a saturated calomel electrode was used as a reference electrode, and a 1 mol / L sulfuric acid aqueous solution was used as an electrolyte. The specific capacitance of the electrode materials prepared in the Examples and Comparative Examples was tested by a constant current charge and discharge method, and the cycle stability of the electrode materials prepared in the Examples and Comparative Examples was tested by cyclic voltammetry, wherein the voltage range was -0.2-0.8V, the charge and discharge current densities were 0.2A / g, 0.5A / g, 1A / g and 2A / g, respectively, and the scan rate was 100mV / s. The test results are shown in Table 1 below.
[0079] Table 1 Performance test results
[0080]
[0081] It can be seen from the above table that the electrode material in the present invention not only has a high discharge specific capacity, which can meet normal practical needs, but also has excellent long-cycle stability. After 1,000 cycles, the capacity retention rate is above 99%, and it has extremely broad application prospects.
[0082] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0083] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A sodium ion lithium battery electrode material, It is characterized in that The raw materials include the following parts by weight: 1-5 parts of modified graphene, 0.1-0.5 parts of dispersant, 0.1-0.5 parts of stabilizer, 3-8 parts of active material, 20-30 parts of composite electrode material, and 60-80 parts of deionized water; The active substance is selected from at least one of hydroxybenzenesulfonic acid, hydroxybenzenesulfonate, and benzenesulfonic acid; The preparation method of the modified graphene is as follows: 1) Add cobalt acetate tetrahydrate, nickel acetate tetrahydrate and polyvinyl pyrrolidone to ethylene glycol, stir at 400-600 r / min for 30-60 min, then add graphene, and continue stirring for 20-50 min to obtain a precursor solution; 2) The precursor solution is transferred to a hydrothermal reactor, and heat-insulated in a hydrothermal oven. After cooling to room temperature, the precipitated precursor is poured into an ethanol solution, ultrasonically shaken at 200-400W for 10-30min, centrifuged and repeatedly washed with deionized water, and the product is frozen and vacuum freeze-dried at -50 to -60°C using a freeze dryer, and then transferred to a muffle furnace for heat-insulation treatment, and naturally cooled to room temperature to obtain modified graphene; In step 1), the usage ratio of cobalt acetate tetrahydrate, nickel acetate tetrahydrate, polyvinyl pyrrolidone, ethylene glycol and graphene is (1-5) g: (0.5-2.5) g: (0.025-0.045) g: (40-60) mL: (5-15) mL; The preparation method of the composite electrode material is as follows: 1) Dissolve tetrabutyl titanate in ethanol solution, stir magnetically for 10-30 minutes to prepare solution A, then grind aluminum nitrate nonahydrate, ammonium dihydrogen phosphate and lithium acetate dihydrate into a paste, add the paste to solution A, stir magnetically at 60-70°C for 1-3 hours, transfer to a muffle furnace for heating treatment, cool to room temperature, and obtain nanoparticles after ball milling for standby use; 2) Nickel nitrate hexahydrate and cobalt nitrate hexahydrate are placed in a container, ethanol solution is added, and magnetic stirring is performed at room temperature for 30-50 minutes to obtain a precursor solution. Ammonia solution is added dropwise to the precursor solution, titrated to a pH of 7.5-8.5, and then allowed to stand for 10-15 hours. The product is repeatedly washed with distilled water and ethanol, filtered, placed in a constant temperature drying oven at 80-90°C and dried for 20-25 hours, and ground to obtain a composite nanomaterial; 3) Mixing the above nanoparticles with the composite nanomaterial to form mixed particles, then evenly mixing with sucrose and adding to an acetone solution, stirring the mixed solution with a magnetic force to make it evenly dispersed until the acetone is completely volatilized, then heating to 600-650°C at 2-5°C / min, keeping the temperature in an argon environment for 3-6 hours, and naturally cooling to room temperature to obtain a composite electrode material; In step 1), the ratio of tetrabutyl titanate, ethanol, aluminum nitrate nonahydrate, ammonium dihydrogen phosphate, and lithium acetate dihydrate is (11.5-15.5) g: (500-800) mL: (2.2-3.0) g: (6.9-8.2) g: (2.9-3.6) g; The muffle furnace heating treatment parameters are as follows: first heat at 450-500°C for 2-5h, then heat to 800-860°C and keep warm for 3-6h; In step 2), the ratio of nickel nitrate hexahydrate to cobalt nitrate hexahydrate and ethanol solution is (5-10) mmol: (2.5-5.0) mmol: (25-50) mL; the concentration of ammonia solution is 0.6-0.8 mol / L; In step 3), the mass ratio of the nanoparticles to the composite nanomaterial is 5:1-3; and the sucrose accounts for 10-30% of the total mass of the mixed particles.
2. The sodium ion lithium battery electrode material according to claim 1, It is characterized in that The dispersant is selected from at least one of hydroxymethyl cellulose, hydroxyethyl cellulose and ethyl cellulose; The stabilizer is selected from at least one of fatty acid zinc, hydrotalcite, and diisooctyl phosphite.
3. The sodium ion lithium battery electrode material according to claim 1, It is characterized in that In step 2), the insulation temperature in the hydrothermal oven is 180-190° C., and the insulation time is 12-15 hours; the insulation temperature in the muffle furnace is 380-420° C., and the insulation time is 2-5 hours.
4. A method for preparing a sodium ion lithium battery electrode material according to any one of claims 1 to 3, It is characterized in that The method comprises the following steps: according to the weight fraction, the modified graphene, the dispersant, the stabilizer, the active substance and the deionized water are stirred and dispersed for 1-5 hours to obtain a dispersion liquid, the dispersion liquid is homogenized for 1-5 times at a pressure of 100-400 MPa, the composite electrode material is added, and the mixture is stirred at a speed of 1000-6000 rpm for 1-5 hours, and after drying, the mixture is heat treated at 200-400° C. for 2-6 hours in a nitrogen atmosphere, and the powder is crushed and sieved to obtain a lithium battery electrode material.