Polyimide composite flakes and preparation method thereof
Polyimide composite floss was prepared through steps such as electrospinning and heating and foaming, which solved the problems of complex processes and difficulty in mass production in the prior art, and achieved efficient and economical preparation of warm floss.
Patent Information
- Application Number
- CN202310896931.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-07-20
AI Technical Summary
It is difficult to quickly and simply prepare composite floss pieces that have the advantages of polyimide nanofibers and polyimide foams in the prior art, and the process is complex and it is difficult to achieve large-scale production.
By preparing polyamic acid spinning fluids A and B, electrospinning is performed to form a nanofiber layer, and alternately receiving is used to form a composite nanofiber membrane, followed by heating foaming and thermal imidation treatment to obtain polyacyl Imine composite floss.
It realizes the simple and rapid preparation of polyimide composite floss pieces, which have good warmth, compression and resilience, and is suitable for the field of cold and warm protection of human bodies.
Smart Images

Figure CN117005106B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of thermal insulation materials, and in particular to a polyimide composite flake and a preparation method thereof. Background Art
[0002] Electrospinning technology has the characteristics of simple manufacturing equipment, low spinning cost, a wide variety of spinnable materials, and strong process controllability. The fiber materials prepared by it have the characteristics of fine diameter, high porosity, small pore size, and light weight. It has great application prospects in the fields of thermal insulation, heat insulation, and sound absorption. However, the nanofibers prepared by electrospinning are usually formed in the form of membranes with low thickness and poor thermal insulation performance.
[0003] Among the types of spinnable materials, polyimide is one of the organic polymer materials with the best comprehensive performance. It has excellent properties such as high and low temperature resistance, flame retardancy, low thermal conductivity, antibacterial, and far infrared. Therefore, the application fields of its nanofiber membrane products and nanofiber flake products are expanding year by year, and the military and civilian markets are broad.
[0004] Wadding refers to a sheet-like material with a fluffy structure made of plant fiber, animal fiber or chemical fiber for warmth, heat insulation or shockproof. In the field of thermal insulation materials for textiles, flakes, as a loose filler, have the advantages of light weight and warmth retention. Wadding is generally prepared by electrospinning in a high humidity environment (humidity greater than 80%). It is usually composed of disordered fiber stacking. After compression, the fluffy structure is easy to collapse, and the tensile properties are poor, and it is highly dependent on the environmental humidity. These problems greatly limit the fiber flakes prepared by electrospinning in actual cold and warmth protection applications.
[0005] So far, there have been many research reports on improving the fluffiness of nanofiber membranes.
[0006] In one study, water mist was applied to the fiber receiving area of electrospinning to obtain fluffy and stacked nanofiber flakes, and then organic solvent vapor was used to dissolve the fiber surface to fuse the adjacent fiber intersections to obtain nanofiber flakes with a certain degree of crosslinking. However, the steam crosslinking time of this technology is long, the process is complicated, and the organic solvent recovery and treatment are difficult, which is not conducive to large-scale production.
[0007] In another study, different concentrations of spinning solutions were spun into microfibers and nanofibers respectively by a cross-type bidirectional electrospinning device, and then received by a positive pressure hot air receiving device, and a cross-linking reaction occurred under the action of hot air, and finally flakes were obtained. However, the process and equipment of this technology are complicated, which is not conducive to large-scale production.
[0008] In addition, polyimide foam is a porous material with gas as the filling phase and polyimide as the matrix. It can store a lot of still air, has the characteristics of low thermal conductivity and low density, has good thermal insulation performance, and has good compressibility and resilience. However, polyimide foam has poor flexibility and feels hard when used directly as a filler, which does not meet people's demand for soft and comfortable thermal insulation sheets.
[0009] Therefore, it is expected to develop a method for preparing a composite flake with simple process and rapid production of the composite flake having both the advantages of polyimide nanofibers and polyimide foams, so as to meet the application requirements in the field of human body cold protection and warmth preservation. Summary of the invention
[0010] Technical issues
[0011] The first object of the present invention is to provide a preparation method which has a simple process and can quickly obtain polyimide composite flakes.
[0012] The second object of the present invention is to provide a fluffy polyimide composite flake, which comprises alternately stacked polyimide nanofiber layers and polyimide foam layers and has good warmth retention, compressibility and resilience.
[0013] Technical Solution
[0014] According to the first invention of the present invention, there is provided a method for preparing a polyimide composite flake, the method comprising the following steps:
[0015] (1) preparing a polyamic acid spinning solution A as a first spinning solution;
[0016] (2) preparing a polyamic acid spinning solution B, adding a chemical foaming agent thereto, and stirring to dissolve the chemical foaming agent to obtain a second spinning solution;
[0017] (3) electrospinning the first spinning solution and the second spinning solution respectively to form a polyamic acid nanofiber layer A and a polyamic acid nanofiber layer B containing a chemical foaming agent, and using a conductive receiving belt to alternately receive the polyamic acid nanofiber layer A and the polyamic acid nanofiber layer B containing a chemical foaming agent to obtain a composite nanofiber membrane comprising the alternately stacked polyamic acid nanofiber layers A and the polyamic acid nanofiber layers B containing a chemical foaming agent, wherein the two outermost layers of the composite nanofiber membrane are both set to the polyamic acid nanofiber layer A;
[0018] (4) heating the composite nanofiber membrane to foam the polyamic acid nanofiber layer B containing a chemical foaming agent and transform it into a polyamic acid foam layer to obtain a polyamic acid composite flake;
[0019] (5) The polyamic acid composite flakes are subjected to thermal imidization treatment to obtain polyimide composite flakes.
[0020] In one embodiment, in step (1),
[0021] The preparation of the polyamic acid spinning solution A comprises: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution A,
[0022] The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenylmethane (MDA), biphenyl diamine (Bz), all-meta-triphenyl diether diamine (1,3,3-APB), 4,4-diaminodiphenyl sulfone (DDS) and 4,4-diamino-2,2-dimethylbiphenyl (DMB),
[0023] The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).
[0024] In one embodiment, in step (2),
[0025] The preparation of the polyamic acid spinning solution B comprises: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution B,
[0026] The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenylmethane (MDA), biphenyl diamine (Bz), all-meta-triphenyl diether diamine (1,3,3-APB), 4,4-diaminodiphenyl sulfone (DDS) and 4,4-diamino-2,2-dimethylbiphenyl (DMB),
[0027] The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).
[0028] The chemical foaming agent is one or more selected from azodicarbonamide, dinitrosopentamethylenetetramine, p-toluenesulfonamidourea, azobisisobutyronitrile, trisaminotriazine and azodicarboxylic acid boron.
[0029] In the second spinning solution, the content of the chemical foaming agent is 0.5-10% of the mass of the polyamic acid in the polyamic acid spinning solution B.
[0030] In one embodiment, in step (3),
[0031] The conductive receiving belt is one or more selected from a non-porous conductive metal belt, a conductive metal porous mesh belt and a fiber belt containing a conductive coating;
[0032] In the composite nanofiber membrane, the ratio of the total mass of all polyamic acid nanofiber layers B containing a chemical foaming agent to the total mass of all polyamic acid nanofiber layers A is 10 to 50%.
[0033] In one embodiment, in step (4),
[0034] The temperature of the heating treatment is 150-250° C., and the time is 0.5-4 hours.
[0035] In one embodiment, in step (5),
[0036] The temperature of the thermal imidization treatment is 300-400° C., and the time is 0.2-3 hours.
[0037] According to a second aspect of the present invention, there is provided a polyimide composite flake prepared by the above method, wherein the polyimide composite flake comprises alternately stacked polyimide nanofiber layers and polyimide foam layers.
[0038] Wherein, the two outermost layers of the polyimide composite flakes are both polyimide nanofiber layers.
[0039] Wherein, the density of the polyimide composite flakes is less than 20 mg / cm 3 , porosity greater than 99%, average pore size less than 2μm, compression rate greater than 70%, and recovery rate greater than 85%.
[0040] Beneficial Effects
[0041] Compared with the prior art, the present invention has the following advantages.
[0042] (1) The flake preparation method of the present invention is simple in process and is not highly dependent on environmental humidity. The present invention replaces the conventional process of preparing nanofiber flakes by electrospinning in a high humidity environment by steps (4) and (5). Therefore, a high humidity environment is not required in the entire process of the present invention.
[0043] (2) In the present invention, in step (2), a chemical foaming agent is added to the polyamic acid spinning solution B to obtain the second spinning solution (ie, the polyamic acid spinning solution B containing the foaming agent).
[0044] Furthermore, in step (3), the present invention obtains a composite nanofiber membrane comprising alternately stacked polyamic acid nanofiber layers A and polyamic acid nanofiber layers B containing a foaming agent by alternately performing electrospinning on the first spinning solution and the second spinning solution, and using a common conductive receiving belt to alternately receive the polyamic acid nanofiber layer A and the polyamic acid nanofiber layer B containing a foaming agent.
[0045] Then, in step (4), a heating and foaming treatment is performed to foam the polyamic acid nanofiber layer containing a chemical foaming agent (volume expansion), and the distance between the polyamic acid nanofiber layers A is increased to form a fluffy polyamic acid composite flake. Further, the polyamic acid nanofiber layer containing a chemical foaming agent is completely converted into a polyamic acid foam layer, and the foaming and expansion further reduces the pore size of the flake, reduces air convection, and thus significantly improves the thermal insulation performance.
[0046] Then, in step (5), during the thermal imidization treatment, the foam structure can be shaped at the same time, thereby giving the composite flakes excellent compressibility and resilience.
[0047] The present invention combines polyimide foam and polyimide nanofiber to obtain a composite flake, which overcomes the problems of poor mechanical properties, flexibility, easy powdering and the like of the existing polyimide foam, while maintaining the excellent thermal insulation performance of the polyimide foam.
[0048] The two outermost layers of the composite batt may be provided as polyimide nanofiber layers, thereby providing comfortable softness.
[0049] (3) In the method of the present invention, a polyamic acid spinning solution A is prepared as the first spinning solution, and a chemical foaming agent is directly added to the polyamic acid spinning solution B to obtain a second spinning solution, and then the first spinning solution and the second spinning solution are respectively subjected to an electrostatic spinning process to prepare nanofibers, and then heated and foamed. The method of the present invention has a simple preparation process, a continuous process flow, and is easy to realize continuous roll production, and has a good industrialization prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] The drawings of this specification show preferred embodiments of the present invention and are used together with the above-mentioned invention content to further illustrate the technical concept of the present invention, so the present invention should not be interpreted as being limited to the contents described in the drawings. At the same time, the shape, size, scale or ratio of the elements in the drawings may be exaggerated for a clearer description.
[0051] Figure 1 The figure is a schematic cross-sectional view of a partial structure of a polyimide composite flake according to one embodiment of the present invention.
[0052] Figure 2a This is a scanning electron microscope (SEM) image of the polyamic acid nanofiber layer B containing a chemical foaming agent in the composite nanofiber membrane obtained in step (3) of Example 1.
[0053] Figure 2b This is a SEM image of the polyimide foam layer of the polyimide composite flakes obtained in step (5) of Example 1.
[0054] Figure 3 This is a SEM image of the polyimide nanofiber layer of the polyimide composite flakes obtained in step (5) of Example 1.
[0055] Reference numerals
[0056] 10 Polyimide nanofiber layer
[0057] 20 Polyimide foam layer DETAILED DESCRIPTION
[0058] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. The terms or words used in this specification and claims should not be restrictively interpreted as common or dictionary definitions, and should be interpreted as meanings and concepts corresponding to the technical ideas of the present invention on the basis that the inventor can appropriately define the concepts of the terms to describe the principles of the invention in the best possible way.
[0059] When the conditions and methods for measuring a property or parameter described in this specification are not described in detail, the property or parameter is measured using the measurement conditions and methods generally used by those skilled in the art.
[0060] Unless otherwise specified, "%" used herein means % by weight.
[0061] Method for preparing polyimide composite flakes
[0062] According to a first aspect of the present invention, there is provided a method for preparing a polyimide composite flake, the method comprising the following steps:
[0063] (1) preparing a polyamic acid spinning solution A as a first spinning solution;
[0064] (2) preparing a polyamic acid spinning solution B, adding a chemical foaming agent thereto, and stirring to dissolve the chemical foaming agent to obtain a second spinning solution;
[0065] (3) electrospinning the first spinning solution and the second spinning solution respectively to form a polyamic acid nanofiber layer A and a polyamic acid nanofiber layer B containing a chemical foaming agent, and using a conductive receiving belt to alternately receive the polyamic acid nanofiber layer A and the polyamic acid nanofiber layer B containing a chemical foaming agent to obtain a composite nanofiber membrane comprising the alternately stacked polyamic acid nanofiber layers A and the polyamic acid nanofiber layers B containing a chemical foaming agent, wherein the two outermost layers of the composite nanofiber membrane are both set to the polyamic acid nanofiber layer A;
[0066] (4) heating the composite nanofiber membrane to foam the polyamic acid nanofiber layer B containing a chemical foaming agent and transform it into a polyamic acid foam layer to obtain a polyamic acid composite flake;
[0067] (5) The polyamic acid composite flakes are subjected to thermal imidization treatment to obtain polyimide composite flakes.
[0068] In the following, each step will be described in detail.
[0069] Step (1) preparing the first spinning solution
[0070] Prepare polyamic acid spinning solution A as the first spinning solution. The polyamic acid spinning solution A can be prepared by conventional methods. For example, a diamine monomer and a dianhydride monomer can be polymerized in a polar solvent, and the polyamic acid spinning solution A can be obtained by reacting for a certain period of time. Suitable diamine monomers and dianhydride monomers and reaction time can be determined according to conventional selection. The molar ratio of the diamine monomer to the dianhydride monomer can be 1:1.
[0071] The diamine monomer is a compound containing two amino groups and is a conventional component for preparing polyamic acid spinning solution. The diamine monomer can be one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenylmethane (MDA), biphenyl diamine (Bz), all-meta-triphenyl diether diamine (1,3,3-APB), 4,4-diaminodiphenyl sulfone (DDS) and 4,4-diamino-2,2-dimethylbiphenyl (DMB).
[0072] The dianhydride monomer is a compound containing two carboxylic anhydride groups and is a conventional component for preparing polyamic acid spinning solution. The dianhydride monomer can be one or more selected from terephthalic anhydride (PMDA), biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).
[0073] The polar solvent may be one or more selected from N,N-dimethylacetamide (DMAC), N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO) and N-methylpyrrolidone (NMP).
[0074] Relative to the total mass of the polyamic acid spinning solution A, the mass fraction of the polyamic acid (ie, the solid content) may be 5 to 50%, preferably 10 to 35%, and more preferably 15 to 25%.
[0075] The reaction time may be 5 to 24 hours, preferably 8 to 22 hours, and more preferably 10 to 20 hours.
[0076] Step (2): Preparing the second spinning solution
[0077] A polyamic acid spinning solution B is prepared, a chemical foaming agent is added thereto, and the solution is stirred to dissolve the chemical foaming agent, thereby obtaining a second spinning solution (ie, the polyamic acid spinning solution B containing the chemical foaming agent).
[0078] The polyamic acid spinning solution B may be prepared in the same manner as in the above step (1), thereby preparing the polyamic acid spinning solution B. The polyamic acid spinning solution B may be the same as or different from the polyamic acid spinning solution A.
[0079] For example, the preparation of the polyamic acid spinning solution B includes: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution B,
[0080] The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenylmethane (MDA), biphenyl diamine (Bz), all-meta-triphenyl diether diamine (1,3,3-APB), 4,4-diaminodiphenyl sulfone (DDS) and 4,4-diamino-2,2-dimethylbiphenyl (DMB).
[0081] The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).
[0082] The chemical foaming agent is generally a solid compound that releases gas after being heated and decomposed, and can form pores in the polymer material. The chemical foaming agent can be one or more selected from azodicarbonamide, dinitrosopentamethylenetetramine, p-toluenesulfonamidourea, azobisisobutyronitrile, trisaminotriazine and azodicarboxylic acid boron.
[0083] The content of the chemical foaming agent can be 0.5-10% of the mass of the polyamic acid in the polyamic acid spinning solution B, preferably 1-8%, and most preferably 3-6%.
[0084] If the content of chemical foaming agent is too low, it will not be easy to foam, resulting in poor foaming effect, thus affecting the fluffiness of the flakes and thus affecting its thermal insulation performance.
[0085] If the content of the chemical foaming agent is too high, the spinnability of the second spinning solution will be affected, which will affect the subsequent electrospinning process.
[0086] There is no particular limitation on the stirring method and stirring time, and the commonly used methods in the art can be used. For example, a stirring rod can be used to stir for 0.5 to 2 hours to completely dissolve the chemical foaming agent in the polyamic acid spinning solution B and mix them evenly to obtain the second spinning solution.
[0087] There is no particular limitation on the order in which steps (1) and (2) are performed. For example, step (1) may be performed first, and then step (2). Alternatively, step (2) may be performed first, and then step (1). Alternatively, steps (1) and (2) may be performed simultaneously.
[0088] Step (3): Preparation of composite nanofiber membrane
[0089] The first spinning solution and the second spinning solution are respectively electrospun to form a polyamic acid nanofiber layer A (hereinafter referred to as layer A) and a polyamic acid nanofiber layer B containing a chemical foaming agent (hereinafter referred to as layer B), and a conductive receiving belt is used to alternately receive the polyamic acid nanofiber layer A and the polyamic acid nanofiber layer B containing a chemical foaming agent to obtain a composite nanofiber membrane comprising the alternatingly stacked polyamic acid nanofiber layers A and the polyamic acid nanofiber layers B containing a chemical foaming agent, wherein the two outermost layers of the composite nanofiber membrane are both set to polyamic acid nanofiber layers A.
[0090] Electrospinning is a simple and effective conventional technology for producing micron- to nanometer-scale fibers. It allows a polymer solution with static electricity to flow and deform in an electrostatic field, and solidify through solvent evaporation to form a fibrous substance.
[0091] There is no particular limitation on the time, speed and material quality of each electrospinning process, which can be appropriately determined according to the specifications of the final composite flakes.
[0092] There is no particular limitation on the number of layers A and B. For example, the number of layers A may be 10 to 100, and the number of layers B may be one less than that of layers A.
[0093] The conductive receiving belt can be one or more selected from a non-porous conductive metal belt, a conductive metal porous mesh belt and a fiber belt containing a conductive coating. The conductive receiving belt is used to receive the layer A and layer B obtained by electrostatic spinning. If a non-conductive receiving belt is used, the layer A and layer B obtained by electrostatic spinning cannot be received.
[0094] Step (4): Preparation of polyamic acid composite flakes
[0095] The composite nanofiber membrane is subjected to a heat treatment to foam the polyamic acid nanofiber layer B containing a chemical foaming agent and transform it into a polyamic acid foam layer, thereby obtaining a polyamic acid composite flake.
[0096] The polyamic acid composite flakes include alternately stacked polyamic acid nanofiber layers and polyamic acid foam layers, wherein the polyamic acid foam layers are derived from the polyamic acid nanofiber layer B containing a chemical foaming agent.
[0097] The chemical foaming method is a method of foaming a polymer material by using a chemical method to generate gas. Specifically, the chemical foaming agent added to the polymer material is heated to decompose the chemical foaming agent and release gas to foam.
[0098] In the present invention, the composite nanofiber membrane is subjected to a heat treatment to foam layer B. The foaming refers to the decomposition of the chemical foaming agent in layer B during the heating process to generate gas, so that the nanofibers in layer B are foamed (volume expansion), and the distance between layers A is increased to form fluffy polyamic acid composite flakes. In addition, by foaming, the chemical foaming agent is completely decomposed, and the layer B is completely transformed into a polyamic acid foam layer. At the same time, the foaming expansion further reduces the pore size of the flakes, reduces air convection, and thus significantly improves the thermal insulation performance.
[0099] The temperature of the heat treatment (ie, the foaming temperature) is 100 to 250°C, preferably 120 to 230°C, and most preferably 150 to 220°C.
[0100] If the foaming temperature is too low, the chemical foaming agent decomposes slowly and cannot produce enough gas, resulting in the expansion force of layer B being too small, which is insufficient to increase the distance between layers A, is not conducive to the storage of static air, and thus affects the thermal insulation performance.
[0101] If the foaming temperature is too high, the chemical foaming agent will decompose too quickly, causing layer B to expand too quickly.
[0102] It is difficult to maintain the foam structure, resulting in rupture and collapse, thus affecting the thermal insulation performance.
[0103] The heating treatment time (i.e., foaming time, which refers to the time for foaming after reaching the foaming temperature at a certain heating rate, the heating rate is generally 5-15°C / min) is 0.5-4 hours, preferably 1-3 hours, for example 1.5-2 hours.
[0104] If the foaming time is too short, the chemical foaming agent is not completely decomposed, and not enough gas is generated during the foaming process to expand layer B to increase the distance between layers A, which is not conducive to the storage of static air, thereby affecting the thermal insulation performance.
[0105] If the foaming time is too long, the process efficiency will be reduced.
[0106] The apparatus for heat treatment is not particularly limited, and for example, an oven may be used.
[0107] Step (5): Preparation of polyimide composite flakes
[0108] The polyamic acid composite flakes are subjected to thermal imidization treatment to obtain polyimide composite flakes.
[0109] The polyimide composite flakes comprise alternately stacked polyimide nanofiber layers and polyimide foam layers, wherein the polyimide nanofiber layers are derived from the polyamic acid nanofiber layers, and the polyimide foam layers are derived from the polyamic acid foam layers.
[0110] Thermal imidization refers to dehydrating and cyclizing polyamic acid at high temperature to obtain polyimide, which is a conventional process for preparing polyimide. Through thermal imidization treatment, both the polyamic acid nanofiber layer and the polyamic acid foam layer can be dehydrated and cyclized to obtain a polyimide nanofiber layer and a polyimide foam layer, respectively. In addition, during the thermal imidization process, the foam structure in the polyimide foam layer can be shaped at the same time to stabilize its structure, thereby giving the composite floccules excellent compressibility and resilience.
[0111] The temperature of thermal imidization may be 300 to 400°C.
[0112] If the temperature is too low, the imidization degree of the polyamic acid nanofibers and the polyamic acid foam will be incomplete, and the resulting composite flakes will be easily degraded, affecting their long-term performance.
[0113] If the temperature is too high, the polyimide composite flakes will undergo thermal decomposition, affecting the performance of the final composite flakes.
[0114] The time of thermal imidization (which refers to the treatment time in a thermal imidization apparatus such as a chain furnace) may be 0.2 to 3 hours, preferably 0.3 to 2 hours, and more preferably 0.5 to 1 hour.
[0115] If the time is too short, the imidization degree of the polyamic acid nanofibers and the polyamic acid foam will be incomplete, and the resulting composite flakes will be easily degraded, resulting in reduced performance of the final flakes.
[0116] If the time is too long, the polyimide composite flakes will undergo thermal decomposition, reducing the quality of the final composite flakes.
[0117] Polyimide composite flakes
[0118] According to a second aspect of the present invention, there is provided a polyimide composite flake, comprising alternately stacked polyimide nanofiber layers and polyimide foam layers, wherein both outermost layers of the polyimide composite flake are polyimide nanofiber layers.
[0119] The polyimide composite flakes can be prepared by the above method of the present invention.
[0120] The density of polyimide composite flakes can be less than 20mg / cm 3 , preferably less than 15 mg / cm 3 , more preferably less than 10 mg / cm 3 ;
[0121] The porosity may be greater than 99%, preferably greater than 99.2%, more preferably greater than 99.5%.
[0122] The average pore size may be less than 2 μm, preferably less than 1.5 μm, more preferably less than 1 μm;
[0123] The compression rate may be greater than 70%, preferably greater than 75%, more preferably greater than 80%;
[0124] The recovery rate may be greater than 85%, preferably greater than 88%, and more preferably greater than 90%.
[0125] There is no particular restriction on the thickness of the polyimide composite flakes. For example, when the composite flakes have a gram weight of 20 g / m 2 In the case of , the thickness can be greater than 1 mm and less than 30 mm.
[0126] The density of the composite flakes can be measured as follows:
[0127] First, the surface density was measured according to GB / T 24218.1-2009 (Test methods for textile nonwovens Part 1: Determination of mass per unit area);
[0128] Then, measure its thickness according to GB / T 24218.2-2009 (Textile nonwoven fabric test methods Part 2: Determination of thickness);
[0129] Next, the density is obtained by dividing the area density by the thickness.
[0130] The porosity of the composite flakes can be calculated according to the mass density method formula: porosity = [1-surface density / (1000*thickness*polyimide density)]*100:
[0131] The unit of surface density is g / m 2 , thickness unit is mm, polyimide density is 1.4g / cm 3 .
[0132] The average pore size of the composite flakes can be measured according to GB / T 42269-2022 (test method for pore size of separation membranes - gas permeation method).
[0133] The compression rate and recovery rate of the composite flakes can be measured according to the test method in Appendix A of FZ / T 64003-2021 (Spray-bonded cotton flakes).
[0134] In one embodiment, the polyimide composite flakes have Figure 1 The partial structure shown, in which the polyimide foam layer 20 is sandwiched between two polyimide nanofiber layers 10.
[0135] Figure 1 Only three layers in the local structure of the composite flake are schematically shown. In the actual composite flake, more layers may be included, for example, 10 to 100 polyimide nanofiber layers 10, and the number of polyimide foam layers 20 is correspondingly one layer less than the number of polyimide nanofiber layers. In addition, the thicknesses of the two polyimide nanofiber layers 10 may be the same or different from each other; the thicknesses of the polyimide nanofiber layer 10 and the polyimide foam layer 20 may also be increased or decreased respectively.
[0136] Example
[0137] Hereinafter, the present invention will be described in detail with reference to embodiments to specifically describe the present invention. However, embodiments of the present invention may be modified into various other forms, and the scope of the present invention should not be construed as being limited to the embodiments described below. Embodiments of the present invention are provided to more fully describe the present invention to those of ordinary skill in the art.
[0138] The experimental methods in the following examples, unless otherwise specified, are generally conventional conditions in the art or conditions recommended by the manufacturer; the raw materials and equipment used are all commercially available from conventional markets, etc., unless otherwise specified.
[0139] The following is based on the same surface density (also known as gram weight, g / m 2 ) Obtain the products of Examples 1 to 6 and Comparative Examples 1 to 2, and compare their thermal insulation properties and other properties.
[0140] Example 1
[0141] The polyimide composite flakes are prepared by a method comprising the following steps.
[0142] Step (1) preparing the first spinning solution
[0143] 200.2 g (1 mol) of diphenyl ether diamine (ODA), 147.1 g (0.5 mol) of biphenyl dianhydride (BPDA), and 109.1 g (0.5 mol) of pyromellitic dianhydride (PMDA) were prepared at a molar ratio of 1:0.5:0.5, and 2228.3 g of N,N-dimethylacetamide (DMAC) as a solvent was also prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A with a solid content (i.e., polyamic acid content) of 17% by mass was obtained as the first spinning solution.
[0144] Step (2): Preparing the second spinning solution
[0145] A polyamic acid spinning solution B was prepared which was the same as the polyamic acid spinning solution A, with a total mass of 1000 g. Then, 5.4 g of azodicarbonamide as a chemical foaming agent was added thereto, and the chemical foaming agent was stirred to dissolve, thereby obtaining a second spinning solution. The content of the chemical foaming agent was 3.2% relative to the mass of the polyamic acid in the polyamic acid spinning solution B.
[0146] Step (3): Preparation of composite nanofiber membrane
[0147] Arrange five groups of electrospinning spinnerets in sequence on a line, and perform electrospinning on the first spinning solution and the second spinning solution.
[0148] The first spinning solution is electrospun in an electric field with an electric field strength of 25 kV / m through the front spinneret group No. 1, the spinneret group No. 3 and the rear spinneret group No. 5.
[0149] The second spinning solution was subjected to electrostatic spinning in an electric field with an electric field strength of 30 kV / m through spinneret group No. 2 and spinneret group No. 4.
[0150] Polyamic acid nanofiber layer A (from the first spinning solution) and polyamic acid nanofiber layer B containing a chemical foaming agent (from the second spinning solution) are alternately formed on a conductive stainless steel belt with a reciprocating speed of 1 m / min. The electrospinning time is 1 hour, and a composite nanofiber membrane with a length of 3 m, a width of 1 m, and a thickness of 600 μm is obtained. The two outermost layers of the composite nanofiber membrane are both set as polyamic acid nanofiber layer A.
[0151] Step (4): Preparation of polyamic acid composite flakes
[0152] The composite nanofiber membrane was placed in an oven and heated to 200° C. at a heating rate of 10° C. / min to allow the polyamic acid nanofiber layer B containing a chemical foaming agent to foam and expand for 1 hour to obtain a polyamic acid composite flake with a thickness of 6 mm.
[0153] Step (5): Preparation of polyimide composite flakes
[0154] The polyamic acid composite flakes are fed into a 5m long chain furnace for thermal imidization treatment. The chain furnace has 5 temperature zones, the temperatures from the inlet end to the outlet end are 100-390°C, and the moving speed of the polyamic acid composite flakes is 0.1m / min.
[0155] The polyimide composite flakes are obtained through the thermal imidization treatment. The two outermost layers of the polyimide composite flakes are both polyimide nanofiber layers.
[0156] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 6mg / cm 3 , thickness is 5mm.
[0157] Example 2 (Using different polyamic acid spinning solutions A and chemical foaming agents to prepare polyimide composite flakes)
[0158] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0159] Step (1) preparing the first spinning solution
[0160] 100.1 g (0.5 mol) of diphenyl ether diamine (ODA), 205.3 g (0.5 mol) of bisphenol A diamine (BAPP), and 218.1 g (1 mol) of pyromellitic dianhydride (PMDA) were prepared at a molar ratio of 0.5:0.5:1, and 2555.9 g of N,N-dimethylacetamide (DMAC) as a solvent were also prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 17% by mass was obtained.
[0161] Step (2): Preparing the second spinning solution
[0162] A polyamic acid spinning solution B was prepared which was the same as the polyamic acid spinning solution A, with a total mass of 1000 g. Then, 5.3 g of dinitrosopentamethylenetetramine as a chemical foaming agent was added thereto, and the chemical foaming agent was stirred to dissolve, thereby obtaining a second spinning solution. The content of the chemical foaming agent was 3.1% relative to the mass of the polyamic acid in the polyamic acid spinning solution B.
[0163] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 5mg / cm 3 , thickness is 6mm.
[0164] Example 3 (Using different polyamic acid spinning solutions A to prepare polyimide composite flakes)
[0165] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0166] Step (1) preparing the first spinning solution
[0167] 160.2 g (0.8 mol) of diphenyl ether diamine (ODA), 42.5 g (0.2 mol) of 4,4-diamino-2,2-dimethylbiphenyl (DMB), 80.5 g (0.2 mol) of triphenyl diether dianhydride (HQPDA), 174.5 g (0.8 mol) of pyromellitic acid dianhydride (PMDA) were prepared in a molar ratio of 0.8:0.2:0.2:0.8, and 2234.7 g of N,N-dimethylacetamide (DMAC) as a solvent were prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 17% by mass was obtained.
[0168] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 5.6mg / cm 3 , thickness is 5.4mm.
[0169] Example 4 (Using different polyamic acid spinning solutions A to prepare polyimide composite flakes)
[0170] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0171] Step (1) preparing the first spinning solution
[0172] 119g (0.6mol) of 4,4-diaminodiphenylmethane (MDA), 164.2g (0.4mol) of bisphenol A diamine (BAPP), 43.6g (0.2mol) of pyromellitic dianhydride (PMDA) and 235.4g (0.8mol) of biphenyl dianhydride (BPDA) were prepared in a molar ratio of 0.6:0.4:0.2:0.8, and 2744.9g of N,N-dimethylacetamide (DMAC) as a solvent was prepared. They were stirred in a reactor for 12h to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 17% by mass was obtained.
[0173] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 5.5mg / cm 3 , thickness is 5.5mm.
[0174] Example 5 (Using different polyamic acid spinning solutions A to prepare polyimide composite flakes)
[0175] The polyimide composite flakes were prepared by the same method as in Example 1, except for the following steps.
[0176] Step (1) preparing the first spinning solution
[0177] 200.2 g (1 mol) of diphenyl ether diamine (ODA), 196.3 g (0.9 mol) of pyromellitic dianhydride (PMDA) and 40.2 g (0.1 mol) of triphenyl diether dianhydride (HQPDA) were prepared in a molar ratio of 1:0.9:0.1, and 2132.1 g of N,N-dimethylacetamide (DMAC) as a solvent was prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 17% by mass was obtained.
[0178] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 5.2mg / cm 3 , thickness is 5.8mm.
[0179] Example 6 (Using different polyamic acid spinning solutions A and chemical foaming agents to prepare polyimide composite flakes)
[0180] The polyimide composite flakes were prepared by the same steps as in Example 1, except for the following steps.
[0181] Step (1) preparing the first spinning solution
[0182] 140.2 g (0.7 mol) of diphenyl ether diamine (ODA), 123.2 g (0.3 mol) of bisphenol A type diamine (BAPP), 152.7 g (0.7 mol) of pyromellitic dianhydride (PMDA) and 156.1 g (0.3 mol) of bisphenol A diether dianhydride (BPADA) were prepared in a molar ratio of 0.7:0.3:0.7:0.3, and 2793.7 g of N,N-dimethylacetamide (DMAC) as a solvent was prepared. They were stirred in a reactor for 12 hours to perform a polymerization reaction, and a polyamic acid spinning solution A having a solid content (i.e., polyamic acid content) of 17% by mass was obtained.
[0183] Step (2): Preparing the second spinning solution
[0184] A polyamic acid spinning solution B is prepared which is the same as the polyamic acid spinning solution A, with a total mass of 1000 g. Then, 6 g of p-toluenesulfonylamide urea as a chemical foaming agent is added thereto, and the chemical foaming agent is stirred to dissolve to obtain a second spinning solution. The content of the chemical foaming agent is 3.5% relative to the mass of the polyamic acid in the polyamic acid spinning solution B.
[0185] The surface density of the obtained polyimide composite flakes is 30g / m 2 , density is 5.7mg / cm 3 , thickness is 5.3mm.
[0186] Comparative Example 1 (blank polyimide nanofiber membrane, not including a polyimide foam layer)
[0187] Only steps (1), (3) and (5) in Example 1 were performed to obtain a blank polyimide nanofiber membrane.
[0188] The surface density of the polyimide nanofiber membrane is 30 g / m 2 , density is 100mg / cm 3 , thickness is 0.3mm.
[0189] Comparative Example 2 (Preparation of Fluffy Polyimide Nanofiber Flakes by High Humidity Environment, Which Does Not Contain a Polyimide Foam Layer)
[0190] Step (1) of Example 1 was carried out to obtain a polyamic acid spinning solution A having a solid content (ie, polyamic acid content) of 17% by mass.
[0191] Then, the polyamic acid spinning solution A was electrospun in an electric field with a humidity of 85% and an electric field strength of 32 kV / m using an electrospinning device containing three groups of spinning nozzles. The polyamic acid nanofibers formed by electrospinning were received by a negatively-voltaged roller, and the electrospinning time was 10 hours to obtain a fluffy polyamic acid nanofiber membrane with a length of 0.8 m, a width of 0.5 m, and a thickness of 4 mm.
[0192] Then, the polyamic acid nanofiber membrane is subjected to step (5) of Example 1 (i.e., thermal imidization treatment) to obtain a polyimide nanofiber flake.
[0193] The surface density of the polyimide nanofiber flakes is 30 g / m 2 , density is 10mg / cm 3 , thickness is 3mm.
[0194] Experimental Example 1: Morphology Observation Using a Scanning Electron Microscope
[0195] A scanning electron microscope (TESCAN, model VEGA3) was used to observe the microstructures of the composite nanofiber membrane obtained in step (3) of Example 1 and the polyimide composite flakes obtained in step (5) according to GB / T36422-2018 (Scanning electron microscopy method for determination of micromorphology and diameter of chemical fibers). Figure 2a , Figure 2b and Figure 3 As shown. Among them,
[0196] Figure 2a is a SEM image of the polyamic acid nanofiber layer B containing a chemical foaming agent;
[0197] Figure 2b is the SEM image of the polyimide foam layer;
[0198] Figure 3 This is the SEM image of the polyimide nanofiber layer.
[0199] from Figure 2a It can be seen that the polyamic acid nanofiber layer B containing a chemical foaming agent and Figure 3 The polyimide nanofiber layer in the film has a similar morphology and presents a three-dimensional network structure.
[0200] from Figure 2b It can be seen that after the polyamic acid nanofiber layer B containing a chemical foaming agent is transformed into a polyimide foam layer through foaming and thermal imidization treatment, its fiber diameter is significantly expanded and coarsened, and its pore size is significantly reduced.
[0201] from Figure 3 It can be seen that the polyimide nanofiber layer in the polyimide composite flakes maintains the morphology of nanofibers and presents a three-dimensional network structure, which can store a large amount of still air.
[0202] Experimental Example 2 Measurement of thermal insulation performance
[0203] The thermal insulation performance of the products of Examples 1 to 6 and Comparative Examples 1 to 2 is compared. The thermal insulation performance of the product is expressed by the Crowe value, which is measured according to GB / T 11048-2008 (Determination of thermal and moisture resistance of textiles under steady-state conditions for physiological comfort).
[0204] Specifically, a fabric thermal insulation performance tester (Wenzhou Darong Textile Instrument Co., Ltd., model YG (B) 606E) was used to measure the Cros values of the products of Examples 1 to 6 and Comparative Examples 1 and 2 according to GB / T 11048-2018. The results are shown in Table 1 below.
[0205] Table 1: Cros values of products
[0206] <![CDATA[Clo value (unit: m 2 ·K / W)]]> Example 1 1.26 Example 2 1.41 Example 3 1.33 Example 4 1.31 Example 5 1.29 Example 6 1.39 Comparative Example 1 0.26 Comparative Example 2 0.83
[0207] As can be seen from Table 1, the polyimide composite flakes of Examples 1 to 6 prepared by the method of the present invention have significantly larger Crowe values, indicating that the warmth retention effect is excellent.
[0208] In particular, it can be seen from the Crowe values of the products of Example 1 and Comparative Example 1 that, for the same polyamic acid raw material, Example 1 can significantly improve the thermal insulation of the obtained flakes by adding a chemical foaming agent for foaming molding.
[0209] Experimental Example 3 Measurement of Average Pore Diameter
[0210] The porosity and average pore size of the products of Examples 1 to 6 and Comparative Examples 1 and 2 were compared.
[0211] The porosity is calculated according to the following mass density method formula:
[0212] Porosity = [1-surface density / (1000*thickness*polyimide density)]*100,
[0213] The unit of surface density is g / m 2 , thickness unit is mm, polyimide density is 1.4g / cm 3 .
[0214] The average pore size was measured according to GB / T 42269-2022 (test method for separation membrane pore size: gas permeation method). Specifically, the average pore size of the products of Examples 1 to 6 and Comparative Examples 1 to 2 was measured using a fully automatic gas permeability meter (Quanta Instruments, USA, model Porometer 3Gzh) according to GB / T 42269-2022.
[0215] The results are shown in Table 2 below.
[0216] Table 2: Porosity and main pore size of the products
[0217] Porosity (%) Average pore size (μm) Example 1 99.57 0.8 Example 2 99.64 1 Example 3 99.60 0.9 Example 4 99.61 0.8 Example 5 99.63 0.9 Example 6 99.60 0.9 Comparative Example 1 92.86 3 Comparative Example 2 99.29 15
[0218] It can be seen from Table 2 that the polyimide composite flakes of Examples 1 to 6 prepared by the method of the present invention have significantly higher porosity and smaller average pore size, which reduces air convection and thus improves thermal insulation performance.
[0219] In particular, it can be seen from the average pore diameters of the products of Example 1 and Comparative Examples 1 to 2 that Example 1 can significantly reduce the average pore diameter of the flakes by adding a chemical foaming agent for foaming molding without affecting the porosity, thereby reducing air convection and improving thermal insulation performance.
[0220] Experimental Example 4 Measurement of Compression Rate and Recovery Rate
[0221] The compression rate and recovery rate of the products of Examples 1 to 6 and Comparative Examples 1 to 2 were measured according to the test method of Appendix A of FZ / T 64003-2021 Spray-bonded Cotton Sheets. The results are shown in Table 3 below.
[0222] Table 3: Compression rate and recovery rate of products
[0223] Compression % Response rate % Example 1 81 90 Example 2 83 91 Example 3 82 90 Example 4 81 91 Example 5 80 91 Example 6 82 92 Comparative Example 1 8 11 Comparative Example 2 80 23
[0224] It can be seen from Table 3 that the polyimide composite flakes of Examples 1 to 6 of the present invention have high compression rates and recovery rates, and are suitable for the field of thermal insulation.
[0225] In comparison, the polyimide nanofiber membrane of Comparative Example 1 has significantly lower compression and recovery rates, poor fluffy structure, and is not suitable for the field of warmth preservation;
[0226] Although the compression rate of the polyimide nanofiber flakes in Comparative Example 2 is relatively high, the recovery rate is significantly low and is not suitable for the field of thermal insulation materials.
[0227] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the present invention.
Claims
1. A method for preparing a polyimide composite flake, the method comprising the following steps: (1) preparing a polyamic acid spinning solution A as a first spinning solution; (2) preparing a polyamic acid spinning solution B, adding a chemical foaming agent thereto, and stirring to dissolve the chemical foaming agent to obtain a second spinning solution; (3) electrospinning the first spinning solution and the second spinning solution respectively to form a polyamic acid nanofiber layer A and a polyamic acid nanofiber layer B containing a chemical foaming agent, and using a conductive receiving belt to alternately receive the polyamic acid nanofiber layer A and the polyamic acid nanofiber layer B containing a chemical foaming agent to obtain a composite nanofiber membrane comprising the alternately stacked polyamic acid nanofiber layers A and the polyamic acid nanofiber layers B containing a chemical foaming agent, wherein the two outermost layers of the composite nanofiber membrane are both set to the polyamic acid nanofiber layer A; (4) heating the composite nanofiber membrane to foam the polyamic acid nanofiber layer B containing a chemical foaming agent and transform it into a polyamic acid foam layer to obtain a polyamic acid composite flake; (5) The polyamic acid composite flakes are subjected to thermal imidization treatment to obtain polyimide composite flakes, wherein the polyamic acid nanofiber layer A is transformed into a polyimide nanofiber layer, and the polyamic acid foam layer is transformed into a polyimide foam layer.
2. The method according to claim 1, wherein: In step (1), The preparation of the polyamic acid spinning solution A comprises: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution A, The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenylmethane (MDA), biphenyl diamine (Bz), all-meta-triphenyl diether diamine (1,3,3-APB), 4,4-diaminodiphenyl sulfone (DDS) and 4,4-diamino-2,2-dimethylbiphenyl (DMB), The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA).
3. The method according to claim 1, wherein: In step (2), The preparation of the polyamic acid spinning solution B comprises: using a diamine monomer and a dianhydride monomer to prepare the polyamic acid spinning solution B, The diamine monomer is one or more selected from diaminodiphenyl ether diamine (ODA), p-phenylenediamine (PPD), bisphenol A diamine (BAPP), 4,4-diaminodiphenylmethane (MDA), biphenyl diamine (Bz), all-meta-triphenyl diether diamine (1,3,3-APB), 4,4-diaminodiphenyl sulfone (DDS) and 4,4-diamino-2,2-dimethylbiphenyl (DMB), The dianhydride monomer is one or more selected from terephthalic anhydride (PMDA), biphenyl dianhydride (BPDA), triphenyl diether dianhydride (HQPDA), diphenyl ether dianhydride (ODPA), benzophenone dianhydride (BTDA), bisphenol A dianhydride (BPADA) and diphenyl sulfide dianhydride (TDPA). The chemical foaming agent is one or more selected from azodicarbonamide, dinitrosopentamethylenetetramine, p-toluenesulfonamidourea, azobisisobutyronitrile, trisaminotriazine and azodicarboxylic acid boron. In the second spinning solution, the content of the chemical foaming agent is 0.5-10% of the mass of the polyamic acid in the polyamic acid spinning solution B.
4. The method according to claim 1, wherein: In step (3), The conductive receiving belt is one or more selected from a non-porous conductive metal belt, a conductive metal porous mesh belt and a fiber belt containing a conductive coating; In the composite nanofiber membrane, the ratio of the total mass of all polyamic acid nanofiber layers B containing a chemical foaming agent to the total mass of all polyamic acid nanofiber layers A is 10 to 50%.
5. The method according to claim 1, wherein: In step (4), The temperature of the heating treatment is 150-250° C., and the time is 0.5-4 hours.
6. The method according to claim 1, wherein: In step (5), The temperature of the thermal imidization treatment is 300-400° C., and the time is 0.2-3 hours.
7. A polyimide composite flake prepared by the method according to claim 1, wherein the polyimide composite flake comprises alternately stacked polyimide nanofiber layers and polyimide foam layers, in, The two outermost layers of the polyimide composite flakes are both polyimide nanofiber layers. Wherein, the density of the polyimide composite flakes is less than 20 mg / cm 3 , porosity greater than 99%, average pore size less than 2μm, compression rate greater than 70%, and recovery rate greater than 85%.
Citation Information
Patent Citations
Composite nanofiber membrane and preparation method and application thereof
CN107299456A
Nanofiber flocculus with sandwich structure and preparation method of nanofiber flocculus
CN111485329A