A graphene-added copper alloy composite material and its preparation method and application
By forming metatungstate ion-copper ion x-gel in copper alloy and subjecting high-temperature calcination and electroless nickel plating, graphene is grown in situ, solving the problem of graphene and metal tungsten reaction, and improving the copper alloy composite material Hardness and conductivity, suitable for a variety of high-performance applications.
Patent Information
- Application Number
- CN202311566576.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-11-22
AI Technical Summary
In the prior art, the reaction and interface bonding of graphene with metal tungsten lead to limited hardness and conductivity of graphene/copper alloy composite materials, and the addition of reinforcements such as rare earth elements reduces the conductivity.
Copper nitrate trihydrate, ammonium metatungstate and citric acid are mixed to form metatungstate-copper ion-dip gel. After high-temperature calcination and electroless nickel plating, graphene is grown in situ under an inert gas atmosphere to form dense copper Tungsten alloy composite material to avoid graphene reacting with metal tungsten.
It significantly improves the hardness and conductivity of the graphene copper alloy composite material, maintains the porous structure and conductivity of the material, and is suitable for high-voltage switching, microelectronics, machinery and aerospace fields.
Smart Images

Figure BDA0004566580070000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of materials, and in particular to a graphene-added copper alloy composite material and a preparation method and application thereof. Background Art
[0002] Tungsten copper alloy has good electrical and thermal conductivity, good high temperature strength, and is widely used in high-voltage switches, microelectronics, machinery, aerospace and other fields. However, with the development of high-voltage power grids towards large capacity and ultra-high voltage, higher requirements are placed on the wear resistance and ablation resistance of tungsten copper alloys. In order to enhance the performance of tungsten copper alloys, the methods reported in the literature include adding a third phase to tungsten copper alloys, such as adding rare earth elements, rare earth oxides (La2O3, ThO2, CeO2) and second phases (HfC, TiC, WC) to tungsten copper alloys to improve the arc ablation performance of tungsten copper alloys. However, it reduces the electrical conductivity of tungsten copper alloys. Therefore, the selection of new reinforcements and the preparation of new tungsten copper alloys are effective measures to improve the comprehensive performance of materials.
[0003] As a new type of material, graphene, a single-layer carbon atom, has excellent mechanical, optical, thermal conductivity, and charge transport properties. In the past decade, there has been an endless stream of research on using graphene as a reinforcement phase to enhance body materials. However, graphene has a low density, is easy to agglomerate, and is very likely to react with metal tungsten during the preparation process, and the interface bonding and other issues can easily restrict the hardness and conductivity of graphene / copper alloy composites.
[0004] Therefore, the present invention solves the above-mentioned problem by improving the preparation process of the copper alloy composite material with added graphene. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides 1. A method for preparing a copper alloy composite material with added graphene, characterized in that it comprises the following preparation steps:
[0006] (1) Copper nitrate trihydrate, ammonium metatungstate and deionized water are fully mixed in a certain proportion, stirred at 400-600 rpm for 40-60 min, then a complexing agent is added, the temperature is raised to 60-80° C., and stirring is continued for 50-70 min to form a sol, and the temperature is further raised to 120° C. to discharge water to form a wet gel, and then heated at 140-160° C. for 23-25 h to form a metatungstate ion-copper ion dry gel;
[0007] (2) after high-temperature calcination in an air atmosphere, immersing in a chemical nickel plating solution at a constant temperature of 85 to 90° C. and a pH value of 4 to 6 for 30 to 60 minutes to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0008] (3) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, and a carbon source gas is introduced under an inert mixed gas atmosphere at a certain temperature and pressure, and the temperature is kept for 5 to 120 minutes to grow graphene, and then it is quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0009] Furthermore, in step (1), the mixing ratio of copper nitrate trihydrate, ammonium metatungstate and deionized water is 1: 0.0018-0.002: 0.5-0.7.
[0010] Furthermore, the complexing agent in step (1) includes citric acid; the added amount of the complexing agent is 0.45 to 0.55 times the mass of copper nitrate trihydrate.
[0011] Furthermore, in step (2), the calcination temperature is controlled at 290-310° C., and the calcination time is 1.9-2.1 h.
[0012] Furthermore, the chemical nickel plating solution in step (2) comprises the following components by weight: 34.9-35.1 wt% nickel nitrate, 29.3-30.5 wt% sodium hypophosphite, 9.4-10.5 wt% lactic acid, 14-16.4 wt% oxalic acid, 4.7-5.2 wt% propionic acid, 0.5 wt% sodium fluoride, and 4.4-4.7 wt% zinc nitrate.
[0013] Furthermore, the inert mixed gas in step (3) is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:8-10.
[0014] Furthermore, the carbon source gas in step (3) includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof; and the flow rate of the carbon source gas is 100 to 200 sccm.
[0015] Furthermore, in step (3), the temperature of the tubular furnace is controlled at 900-1150° C., and the pressure is controlled at 20-200 Pa.
[0016] The present invention also provides a graphene-added copper alloy composite material, wherein the graphene-added copper alloy composite material is prepared by adopting the preparation method of the graphene-added copper alloy composite material.
[0017] The present invention also provides an application of a copper alloy composite material with added graphene, and the copper alloy composite material with added graphene can be applied to high-voltage switches, microelectronics, machinery and aerospace fields.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The invention discloses a copper alloy composite material added with graphene, and a preparation method and application thereof. Firstly, copper nitrate trihydrate, ammonium metatungstate and complexing agent citric acid are mixed to form a metatungstate ion-copper ion dry gel; then, the metatungstate ion-copper ion dry gel is subjected to high-temperature calcination at 290-310 DEG C and chemical nickel plating to obtain a nickel-plated metatungstate ion-copper ion dry gel; finally, in the presence of an inert mixed gas of hydrogen and argon, graphene is in situ grown in the nickel-plated metatungstate ion-copper ion dry gel to obtain the copper alloy composite material added with graphene.
[0020] Copper nitrate trihydrate, ammonium metatungstate, and citric acid are mixed to form a metatungstate ion-copper ion dry gel network, which disperses the strengthening phase tungsten into copper, refines the copper grains, and enhances the hardness and conductivity of the copper alloy composite material with added graphene; after calcining the metatungstate ion-copper ion dry gel network at 290-310°C, the copper and tungsten composite oxides are formed while maintaining the gel network of the metatungstate ion-copper ion dry gel and the fluffy porous structure, followed by chemical nickel plating to coat the surface of the copper and tungsten composite oxide particles with a nickel layer. , which can prevent the subsequent reaction of graphene with metal tungsten, is beneficial to the subsequent sintering of copper-tungsten alloy. In the inert mixed gas of hydrogen and argon, the carbon source gas quickly enters the fluffy and porous nickel-plated metatungstate ion-copper ion dry gel, forms graphene in situ in the pores, and evenly disperses the graphene in the fluffy and porous nickel-plated metatungstate ion-copper ion dry gel. The copper and tungsten composite oxides are reduced to form a copper-tungsten alloy, and a dense copper alloy composite material with added graphene is obtained, which further enhances the hardness and conductivity of the copper alloy composite material with added graphene. DETAILED DESCRIPTION
[0021] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the copper alloy composite material with added graphene prepared in the following examples as follows:
[0022] Hardness: The copper alloy composite materials with added graphene prepared in the embodiment and the comparative example with the same mass were tested for Brinell hardness according to GB / T 231.1-2018.
[0023] Electrical conductivity: The electrical conductivity of the copper alloy composite material with added graphene prepared in the embodiment and the comparative example of the same mass was tested according to GB / T32791-2016.
[0024] Example 1
[0025] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0026] (1) Mix copper nitrate trihydrate, ammonium metatungstate and deionized water in a mass ratio
[0027] 1:0.0018:0.5 was fully mixed, stirred at 400 rpm for 40 min, and then 0.45 times the mass of copper nitrate trihydrate as a complexing agent citric acid was added, and then the temperature was raised to 60°C, and the stirring was continued for 50 min, and the temperature was further raised to 120°C to discharge the water to form a wet gel, and then heated at 140°C for 23 h to obtain a metatungstate ion-copper ion dry gel;
[0028] (2) In an air atmosphere, the metatungstate ion-copper ion xerogel was calcined at 290° C. for 2 h, and then immersed in a chemical nickel plating solution at a constant temperature of 85° C. and a pH value of 4 for 30 min to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0029] (3) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, the temperature is raised to 900°C, 100 sccm of carbon source gas is introduced under an inert mixed gas atmosphere of 20 Pa, the temperature is kept for 5 minutes, graphene is grown, and then it is quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0030] The chemical nickel plating solution includes, by weight, 34.9 wt % nickel nitrate, 29.3 wt % sodium hypophosphite, 9.4 wt % lactic acid, 16.4 wt % oxalic acid, 5.2 wt % propionic acid, 0.5 wt % sodium fluoride, and 4.7 wt % zinc nitrate.
[0031] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:8.
[0032] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0033] Example 2
[0034] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0035] (1) Copper nitrate trihydrate, ammonium metatungstate, and deionized water were fully mixed in a mass ratio of 1:0.0019:0.6, stirred at 500 rpm for 50 min, and then 0.5 times the mass of copper nitrate trihydrate as a complexing agent, citric acid, was added, and then the temperature was raised to 70°C, and the stirring was continued for 60 min, and the temperature was further raised to 120°C to discharge water to form a wet gel, and then heated at 150°C for 24 h to obtain a metatungstate ion-copper ion dry gel;
[0036] (2) In an air atmosphere, the metatungstate ion-copper ion xerogel was calcined at 300° C. for 2 h, and then immersed in a chemical nickel plating solution at a constant temperature of 87° C. and a pH value of 5 for 45 min to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0037] (3) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, heated to 1000°C, and 150sccm of carbon source gas is introduced under an inert mixed gas atmosphere of 100Pa. The temperature is kept for 60 minutes to grow graphene, and then quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0038] The chemical nickel plating solution comprises, by weight, 35 wt % nickel nitrate, 29.9 wt % sodium hypophosphite, 9.9 wt % lactic acid, 15.2 wt % oxalic acid, 5 wt % propionic acid, 0.5 wt % sodium fluoride and 4.5 wt % zinc nitrate.
[0039] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:9.
[0040] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0041] Example 3
[0042] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0043] (1) Copper nitrate trihydrate, ammonium metatungstate, and deionized water were fully mixed in a mass ratio of 1:0.002:0.7, stirred at 600 rpm for 60 min, and then 0.55 times the mass of copper nitrate trihydrate as a complexing agent citric acid was added, and then the temperature was raised to 80°C, and the stirring was continued for 70 min, and the temperature was further raised to 120°C to discharge water to form a wet gel, and then heated at 160°C for 25 h to obtain a metatungstate ion-copper ion dry gel;
[0044] (2) In an air atmosphere, the metatungstate ion-copper ion xerogel was calcined at 310° C. for 2 h, and then immersed in a chemical nickel plating solution at a constant temperature of 90° C. and a pH value of 6 for 60 min to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0045] (3) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, the temperature is raised to 1150°C, 200 sccm of carbon source gas is introduced under an inert mixed gas atmosphere of 200 Pa, the temperature is kept for 120 minutes, graphene is grown, and then it is quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0046] The chemical nickel plating solution includes, by weight, 35.1 wt % nickel nitrate, 30.5 wt % sodium hypophosphite, 10.5 wt % lactic acid, 14 wt % oxalic acid, 5.2 wt % propionic acid, 0.5 wt % sodium fluoride, and 4.4 wt % zinc nitrate.
[0047] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:10.
[0048] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0049] Comparative Example 1
[0050] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0051] (1) Copper nitrate trihydrate, ammonium metatungstate, and deionized water were fully mixed in a mass ratio of 1:0.0019:0.6, stirred at 500 rpm for 50 min, and then 0.5 times the mass of copper nitrate trihydrate as a complexing agent, citric acid, was added, and then the temperature was raised to 70°C, and the stirring was continued for 60 min, and the temperature was further raised to 120°C to discharge water to form a wet gel, and then heated at 150°C for 24 h to obtain a metatungstate ion-copper ion dry gel;
[0052] (2) In an air atmosphere, the metatungstate ion-copper ion xerogel was calcined at 200° C. for 2 h, and then immersed in a chemical nickel plating solution at a constant temperature of 87° C. and a pH value of 5 for 45 min to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0053] (3) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, heated to 1000°C, and 150sccm of carbon source gas is introduced under an inert mixed gas atmosphere of 100Pa. The temperature is kept for 60 minutes to grow graphene, and then quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0054] The chemical nickel plating solution comprises, by weight, 35 wt % nickel nitrate, 29.9 wt % sodium hypophosphite, 9.9 wt % lactic acid, 15.2 wt % oxalic acid, 5 wt % propionic acid, 0.5 wt % sodium fluoride and 4.5 wt % zinc nitrate.
[0055] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:9.
[0056] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0057] Comparative Example 2
[0058] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0059] (1) Copper nitrate trihydrate, ammonium metatungstate, and deionized water were fully mixed in a mass ratio of 1:0.0019:0.6, stirred at 500 rpm for 50 min, and then 0.5 times the mass of copper nitrate trihydrate as a complexing agent, citric acid, was added, and then the temperature was raised to 70°C, and the stirring was continued for 60 min, and the temperature was further raised to 120°C to discharge water to form a wet gel, and then heated at 150°C for 24 h to obtain a metatungstate ion-copper ion dry gel;
[0060] (2) In an air atmosphere, the metatungstate ion-copper ion xerogel was calcined at 400° C. for 2 h, and then immersed in a chemical nickel plating solution at a constant temperature of 87° C. and a pH value of 5 for 45 min to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0061] (3) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, heated to 1000°C, and 150sccm of carbon source gas is introduced under an inert mixed gas atmosphere of 100Pa. The temperature is kept for 60 minutes to grow graphene, and then quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0062] The chemical nickel plating solution comprises, by weight, 35 wt % nickel nitrate, 29.9 wt % sodium hypophosphite, 9.9 wt % lactic acid, 15.2 wt % oxalic acid, 5 wt % propionic acid, 0.5 wt % sodium fluoride and 4.5 wt % zinc nitrate.
[0063] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:9.
[0064] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0065] Comparative Example 3
[0066] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0067] (1) Copper nitrate trihydrate, ammonium metatungstate, and deionized water were fully mixed in a mass ratio of 1:0.0019:0.6, stirred at 500 rpm for 50 min, and then 0.5 times the mass of copper nitrate trihydrate as a complexing agent, citric acid, was added, and then the temperature was raised to 70°C, and the stirring was continued for 60 min, and the temperature was further raised to 120°C to discharge water to form a wet gel, and then heated at 150°C for 24 h to obtain a metatungstate ion-copper ion dry gel;
[0068] (2) In an air atmosphere, the metatungstate ion-copper ion dry gel was calcined at 300°C for 2h, then placed in a tubular furnace, heated to 1000°C, and introduced with 150sccm of carbon source gas in an inert mixed gas atmosphere at 100Pa for 60min to grow graphene, and then quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0069] The chemical nickel plating solution comprises, by weight, 35 wt % nickel nitrate, 29.9 wt % sodium hypophosphite, 9.9 wt % lactic acid, 15.2 wt % oxalic acid, 5 wt % propionic acid, 0.5 wt % sodium fluoride and 4.5 wt % zinc nitrate.
[0070] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:9.
[0071] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0072] Comparative Example 4
[0073] A method for preparing a graphene-added copper alloy composite material comprises the following preparation steps:
[0074] (1) tungsten powder with a particle size of 12 μm and electrolytic copper powder with a particle size of 80 μm were mixed in a mass ratio of 6:94, and then calcined at 300° C. for 2 h in an air atmosphere, and then immersed in a chemical nickel plating solution at a constant temperature of 87° C. and a pH value of 5 for 45 min to obtain a nickel-plated metatungstate ion-copper ion xerogel;
[0075] (2) The nickel-plated metatungstate ion-copper ion dry gel is placed in a tubular furnace, heated to 1000°C, and 150sccm of carbon source gas is introduced under an inert mixed gas atmosphere of 100Pa. The temperature is kept for 60 minutes to grow graphene, and then quickly cooled to room temperature to obtain a copper alloy composite material with added graphene.
[0076] The chemical nickel plating solution comprises, by weight, 35 wt % nickel nitrate, 29.9 wt % sodium hypophosphite, 9.9 wt % lactic acid, 15.2 wt % oxalic acid, 5 wt % propionic acid, 0.5 wt % sodium fluoride and 4.5 wt % zinc nitrate.
[0077] The inert mixed gas is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:9.
[0078] The carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof.
[0079] Effect example
[0080] Table 1 below shows the analysis results of hardness and electrical conductivity of the copper alloy composite materials with added graphene prepared by Examples 1 to 3 of the present invention and Comparative Examples 1 to 4.
[0081] Table 1
[0082]
[0083] From Table 1, it can be found that the copper alloy composite materials with added graphene obtained in Examples 1, 2, and 3 have good hardness and conductivity; from the comparison of the experimental data of Examples 1, 2, and 3 and Comparative Examples 1 and 2, it can be found that the calcination temperature of the metatungstate ion-copper ion dry gel is controlled at 290-310°C, and the obtained copper alloy composite materials with added graphene have good hardness and good conductivity; from the experimental data of Examples 1, 2, and 3 and Comparative Example 3, it can be found that the metatungstate ion-copper ion dry gel after high-temperature calcination is chemically nickel-plated, and the obtained copper alloy composite materials with added graphene have good hardness and good conductivity; from the experimental data of Examples 1, 2, and 3 and Comparative Example 4, it can be found that the copper alloy composite materials with added graphene prepared by using the metatungstate ion-copper ion dry gel as a tungsten-copper alloy raw material have good hardness and good conductivity.
[0084] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a copper alloy composite material with added graphene, characterized in that: The method comprises the following preparation steps: (1) Copper nitrate trihydrate, ammonium metatungstate and deionized water are fully mixed in a certain proportion, and then a complexing agent is added. After heating and mixing, a sol is formed, and after heating for multiple times, a metatungstate ion-copper ion xerogel is formed; (2) calcining at high temperature in an air atmosphere and immersing in a chemical nickel plating solution for chemical nickel plating to obtain a nickel-plated metatungstate ion-copper ion xerogel; (3) placing the nickel-plated metatungstate ion-copper ion xerogel into a tubular furnace, introducing a carbon source gas under an inert mixed gas atmosphere at a certain temperature and pressure, and obtaining a copper alloy composite material with added graphene; The mixing ratio of copper nitrate trihydrate, ammonium metatungstate and deionized water in step (1) is: 1: 0.0018-0.002: 0.5-0.7; The complexing agent in step (1) includes citric acid; the amount of the complexing agent added is 0.45 to 0.55 times the mass of copper nitrate trihydrate; The calcination temperature in step (2) is controlled at 290-310° C. and the calcination time is 1.9-2.1 h; The chemical nickel plating solution in step (2) comprises the following components by weight: 34.9-35.1 parts of nickel nitrate, 29.3-30.5 parts of sodium hypophosphite, 9.4-10.5 parts of lactic acid, 14-16.4 parts of oxalic acid, 4.7-5.2 parts of propionic acid, 0.5 parts of sodium fluoride, and 4.4-4.7 parts of zinc nitrate; the chemical nickel plating solution is kept at a constant temperature of 85-90° C. and has a pH value of 4-6; In step (3), the temperature of the tube furnace is controlled at 900-1150° C., and the pressure is controlled at 20-200 Pa. In step (3), the carbon source gas includes methane, acetylene, ethane, propane, ethylene, propylene, propyne, or a combination thereof; and the flow rate of the carbon source gas is 100-200 sccm.
2. The method for preparing the copper alloy composite material with added graphene according to claim 1, characterized in that: The inert mixed gas in step (3) is a mixture of hydrogen and argon, wherein the mass ratio of hydrogen to argon is 1:8-10.
3. A graphene-added copper alloy composite material prepared according to the preparation method according to any one of claims 1 to 2.
Citation Information
Patent Citations
Preparation method of graphene-doped tungsten-copper alloy
CN106498209A
Tungsten-dispersion strengthened copper-based composite material and preparation method thereof
CN108251685A