A high temperature acidification corrosion inhibitor

CN117512600BActive Publication Date: 2024-11-22ANHUI RED SUN NEW MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202311411115.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-28
Publication Date
2024-11-22
Estimated Expiration
2043-10-28

AI Technical Summary

Technical Problem

The existing corrosion inhibitors are not effective in high temperature and acidic environments, and cannot effectively slow down the corrosion rate of metals, affecting oil collection efficiency and equipment life.

Method used

High-temperature acidification corrosion inhibitor composed of pyridine quaternary ammonium salt, vinylbenzyl trimethyl ammonium chloride grafted carboxymethyl chitosan, propynol, triethanolamine and surfactant are improved by graft copolymerization. Film-forming and dispersible, suitable for deep well mining of high-temperature oil fields at 100-120℃.

Benefits of technology

In high-temperature acidic media, the stability and corrosion resistance of corrosion inhibitors are significantly improved, the oil industry standards are met, the equipment service life is extended, and the production costs and environmental pollution are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004518295970000051
    Figure BDA0004518295970000051
Patent Text Reader

Abstract

The invention discloses a high-temperature acidification corrosion inhibitor, comprising the following raw materials in mass percentage: 10-15% of quaternary ammonium pyridine salt, 5-10% of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, 2-3% of propargyl alcohol, 2-5% of triethanolamine, 0.5-1% of surfactant, and the balance being solvent. The corrosion inhibitor of the invention has good dispersibility and stability in an acidic medium at high temperature, and has excellent high-temperature corrosion resistance, and can meet the use requirements of deep well mining engineering in oil fields at high temperatures of 100-120°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of corrosion inhibitors, in particular to a high-temperature acidification corrosion inhibitor. Background Art

[0002] In the exploration and exploitation of oil, a large number of drilling equipment, transportation pipelines, etc. are needed. Since the environment of the oil field is often very complex and harsh, including high temperature and acidic environment, this high temperature and acidic environment can easily corrode the oil well equipment and pipelines, thereby affecting the oil collection efficiency and the service life of the equipment. Generally speaking, in order to reduce the corrosion of equipment and pipelines, the method of adding corrosion inhibitors during the production process can be adopted. Corrosion inhibitors can greatly slow down the corrosion rate of metals, extend the service life of equipment, and reduce production hazards and environmental pollution caused by equipment corrosion. It not only saves equipment renewal costs and reduces production costs, but also greatly reduces the harm to the ecological environment. However, the usual corrosion inhibitors are used in normal temperature environments. Under high temperature and acidic conditions, due to the influence of special environmental factors, there is often a problem that the corrosion inhibition effect cannot achieve the expected effect. Therefore, the development of corrosion inhibitors suitable for high temperature and acidic environments has very important application significance. Summary of the invention

[0003] Based on the technical problems existing in the background technology, the present invention proposes a high-temperature acidification corrosion inhibitor.

[0004] The invention provides a high temperature acidification corrosion inhibitor, which comprises the following raw materials in percentage by mass: 10-15% of quaternary ammonium pyridine salt, 5-10% of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, 2-3% of propargyl alcohol, 2-5% of triethanolamine, 0.5-1% of surfactant and the balance of solvent.

[0005] Preferably, the preparation method of the quaternary ammonium salt of pyridine is: dissolving 4-methylpyridine and benzyl chloride in an appropriate amount of water, reacting at 80-90° C. for 3-5 hours under an inert atmosphere to obtain the quaternary ammonium salt.

[0006] Preferably, the molar ratio of 4-methylpyridine to benzyl chloride is 1:(1-1.5).

[0007] Preferably, in the method for preparing quaternary ammonium salt of pyridine, the mass ratio of 4-methylpyridine to water is 1:(2.5-3.5).

[0008] Preferably, the preparation method of the vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan is: add carboxymethyl chitosan to an appropriate amount of water, first stir at 50-90°C for 1-2h, then add vinylbenzyltrimethylammonium chloride and an initiator, and stir and react at 80-90°C under an inert atmosphere for 6-12h to obtain the product.

[0009] Preferably, the mass ratio of carboxymethyl chitosan, vinylbenzyltrimethylammonium chloride and initiator is 1:(2-4):(0.01-0.05).

[0010] Preferably, the initiator is ammonium persulfate.

[0011] Preferably, in the method for preparing vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, the mass ratio of carboxymethyl chitosan to water is 1:(10-20).

[0012] Preferably, the surfactant is at least one of emulsifier OP-10, nonylphenol polyoxypropylene ether, and Tween-80.

[0013] Preferably, the solvent is at least one of isopropanol, n-butanol, ethyl ether, propylene oxide, ethylene glycol methyl ether, ethylene glycol diethyl ether, acetonitrile and N,N-dimethylformamide.

[0014] The beneficial effects of the present invention are as follows:

[0015] The present invention grafts vinylbenzyltrimethylammonium chloride onto carboxymethyl chitosan molecules by graft copolymerization, and obtains a carboxymethyl chitosan quaternary ammonium salt containing benzyl and quaternary ammonium groups, and compounding the quaternary ammonium salt of pyridine synthesized by 4-methylpyridine and benzyl chloride has excellent stability and film-forming properties at high temperatures, can be firmly adsorbed on the metal surface, and the high content of benzyl groups in the corrosion inhibitor is also conducive to improving the hydrophobic properties of the corrosion inhibitor film and enhancing the corrosion inhibition effect. The corrosion inhibitor of the present invention has good dispersibility and stability in an acidic medium at high temperature, and has excellent high temperature corrosion resistance, and can meet the use requirements of deep well mining engineering in oil fields at high temperatures of 100-120°C. DETAILED DESCRIPTION

[0016] The technical solution of the present invention is described in detail below through specific embodiments.

[0017] Example 1

[0018] A high-temperature acidification corrosion inhibitor comprises the following raw materials in percentage by mass: 12% of quaternary ammonium pyridine salt, 8% of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, 2.5% of propargyl alcohol, 3% of triethanolamine, 0.8% of Tween-80, and the balance is isopropanol.

[0019] in:

[0020] The preparation method of pyridine quaternary ammonium salt is as follows: 4-methylpyridine and benzyl chloride are dissolved in water, and reacted at 85°C for 4 hours under a nitrogen atmosphere to obtain the quaternary ammonium salt; the molar ratio of 4-methylpyridine to benzyl chloride is 1:1.4; and the mass ratio of 4-methylpyridine to water is 1:3.

[0021] The preparation method of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan is as follows: add carboxymethyl chitosan into water, stir at 60°C for 1.5h, then add vinylbenzyltrimethylammonium chloride and ammonium persulfate, stir and react at 85°C under nitrogen atmosphere for 10h, and obtain the product; wherein the mass ratio of carboxymethyl chitosan, vinylbenzyltrimethylammonium chloride and ammonium persulfate is 1:3:0.03, and the mass ratio of carboxymethyl chitosan to water is 1:15.

[0022] Example 2

[0023] A high-temperature acidification corrosion inhibitor comprises the following raw materials in percentage by mass: 10% of quaternary ammonium pyridine salt, 10% of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, 2% of propargyl alcohol, 5% of triethanolamine, 1% of Tween-80, and the balance is n-butanol.

[0024] in:

[0025] The preparation method of pyridine quaternary ammonium salt is as follows: 4-methylpyridine and benzyl chloride are dissolved in water, and reacted at 80°C for 5 hours under a nitrogen atmosphere to obtain the quaternary ammonium salt; the molar ratio of 4-methylpyridine to benzyl chloride is 1:1; and the mass ratio of 4-methylpyridine to water is 1:2.5.

[0026] The preparation method of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan is as follows: add carboxymethyl chitosan into water, stir at 50°C for 2h, then add vinylbenzyltrimethylammonium chloride and ammonium persulfate, stir and react at 80°C under nitrogen atmosphere for 12h, and obtain the product; wherein the mass ratio of carboxymethyl chitosan, vinylbenzyltrimethylammonium chloride and ammonium persulfate is 1:2:0.01, and the mass ratio of carboxymethyl chitosan to water is 1:10.

[0027] Example 3

[0028] A high-temperature acidification corrosion inhibitor comprises the following raw materials in percentage by mass: 15% of quaternary ammonium pyridine salt, 5% of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, 3% of propargyl alcohol, 2% of triethanolamine, 0.5% of emulsifier OP-10, and the balance of N,N-dimethylformamide.

[0029] in:

[0030] The preparation method of pyridine quaternary ammonium salt is as follows: 4-methylpyridine and benzyl chloride are dissolved in water, and reacted at 90° C. for 3 hours under a nitrogen atmosphere to obtain the quaternary ammonium salt; the molar ratio of 4-methylpyridine to benzyl chloride is 1:1.5; and the mass ratio of 4-methylpyridine to water is 1:3.5.

[0031] The preparation method of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan is as follows: add carboxymethyl chitosan into water, stir at 90°C for 1 hour, then add vinylbenzyltrimethylammonium chloride and ammonium persulfate, stir and react at 90°C for 6 hours under a nitrogen atmosphere to obtain the obtained product; wherein the mass ratio of carboxymethyl chitosan, vinylbenzyltrimethylammonium chloride and ammonium persulfate is 1:4:0.05, and the mass ratio of carboxymethyl chitosan to water is 1:20.

[0032] Comparative Example 1

[0033] A corrosion inhibitor comprises the following raw materials in percentage by mass: 12% of quaternary ammonium pyridine salt, 8% of carboxymethyl chitosan, 2.5% of propargyl alcohol, 3% of triethanolamine, 0.8% of Tween-80, and the balance is isopropanol.

[0034] The preparation method of pyridine quaternary ammonium salt is as follows: 4-methylpyridine and benzyl chloride are dissolved in water, and reacted at 85°C for 4 hours under a nitrogen atmosphere to obtain the quaternary ammonium salt; the molar ratio of 4-methylpyridine to benzyl chloride is 1:1.4; and the mass ratio of 4-methylpyridine to water is 1:3.

[0035] Comparative Example 2

[0036] A corrosion inhibitor comprises the following raw materials in percentage by mass: 20% of quaternary ammonium pyridine salt, 2.5% of propargyl alcohol, 3% of triethanolamine, 0.8% of Tween-80, and the balance is isopropanol.

[0037] The preparation method of pyridine quaternary ammonium salt is as follows: 4-methylpyridine and benzyl chloride are dissolved in water, and reacted at 85°C for 4 hours under a nitrogen atmosphere to obtain the quaternary ammonium salt; the molar ratio of 4-methylpyridine to benzyl chloride is 1:1.4; and the mass ratio of 4-methylpyridine to water is 1:3.

[0038] Test example

[0039] The corrosion inhibition performance of the corrosion inhibitors prepared in Example 1 and Comparative Examples 1-2 in high temperature and acidic medium was tested with reference to the standard of SY / T5405-1996 "Test Methods and Evaluation Indicators for Acidification Corrosion Inhibitors". The test conditions are: corrosion inhibitor concentration 1%, temperature 120°C, corrosion time 4h, test piece N80 steel sheet, acid solution 20wt% HCl solution. The test results are shown in Table 1:

[0040] Table 1

[0041]

[0042] As can be seen from Table 1, the corrosion inhibitor of the present invention can meet the first-level index of the petroleum industry standard SY / T5405-1996 under the condition of 120°C, has excellent high temperature corrosion resistance, and can meet the use requirements of deep well mining projects in oil fields at high temperatures of 100-120°C.

[0043] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high temperature acidification corrosion inhibitor, It is characterized in that The method comprises the following raw materials in percentage by weight: 10-15% of quaternary ammonium pyridine salt, 5-10% of vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan, 2-3% of propargyl alcohol, 2-5% of triethanolamine, 0.5-1% of surfactant, and the balance being solvent; The preparation method of the pyridine quaternary ammonium salt is as follows: 4-methylpyridine and benzyl chloride are dissolved in an appropriate amount of water, and reacted at 80-90° C. for 3-5 hours under an inert atmosphere to obtain the quaternary ammonium salt; the molar ratio of 4-methylpyridine to benzyl chloride is 1:(1-1.5); The preparation method of the vinylbenzyltrimethylammonium chloride grafted carboxymethyl chitosan is as follows: add carboxymethyl chitosan to an appropriate amount of water, stir at 50-90°C for 1-2h, then add vinylbenzyltrimethylammonium chloride and an initiator, stir and react at 80-90°C under an inert atmosphere for 6-12h to obtain the obtained product; the mass ratio of carboxymethyl chitosan, vinylbenzyltrimethylammonium chloride and initiator is 1:(2-4):(0.01-0.05).

2. The high temperature acidification corrosion inhibitor according to claim 1, It is characterized in that The initiator is ammonium persulfate.

3. The high temperature acidification corrosion inhibitor according to claim 1, It is characterized in that The surfactant is at least one of emulsifier OP-10, nonylphenol polyoxypropylene ether and Tween-80.

4. The high temperature acidification corrosion inhibitor according to claim 1, It is characterized in that The solvent is at least one of isopropanol, n-butanol, ethyl ether, propylene oxide, ethylene glycol methyl ether, ethylene glycol diethyl ether, acetonitrile and N,N-dimethylformamide.

Citation Information

Patent Citations

  • The preparation method and application of a Mannich base quaternary ammonium salt

    AU2021100133A4

  • Corrosion inhibitor and preparation method thereof

    CN103289671A

  • Corrosion inhibitor applicable to crosslinked acid acidification at 120-140 DEG C and preparation method of corrosion inhibitor applicable to crosslinked acid acidification at 120-140 DEG C

    CN106350056A

  • Compound high-temperature acidizing corrosion inhibitor based on pyridine quaternary ammonium salt

    CN107523287A

  • Corrosion inhibitor and preparation method thereof

    CN109868478A