A high-strength antibacterial titanium alloy material for additive manufacturing and its preparation method and application

By rationally formulating titanium alloy materials containing Mo, Zr, Fe, and Cu elements in additive manufacturing technology, the problems of high elastic modulus and biological inertness of traditional titanium alloy materials are solved, and high-strength antibacterial properties and biocompatibility are achieved. Improved, suitable for a variety of additive manufacturing technologies.

CN117568658BActive Publication Date: 2024-10-01GUANGDONG INST OF NEW MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311591509.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-10-01
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

The elastic modulus of traditional titanium alloy materials is too high, resulting in insufficient load-bearing pressure of bone tissue, and poor biological inertness and antibacterial properties, leading to nosocomial infection problems; the existing antibacterial titanium alloy preparation methods are complex, the structure is uneven, and the stability is poor.

Method used

Additive manufacturing technology is used to prepare high-strength antibacterial titanium alloy materials, containing Mo, Zr, Fe, and Cu elements. Ti-Mo-Zr-Fe alloy powder is prepared through vacuum air atomization and ball milled with pure copper powder to form Ti-Mo-Zr. -Fe-xCu powder, used for laser 3D printing, regulates the proportion of Cu element to reduce elastic modulus and improve biocompatibility.

Benefits of technology

The material's low modulus, antibacterial properties and biocompatibility have been improved, and the tissue uniformity and stability have been improved. It is suitable for various additive manufacturing technologies such as laser selective melting and selective laser sintering, and has expanded the use scope of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117568658B_ABST
    Figure CN117568658B_ABST
Patent Text Reader

Abstract

The present invention provides a high-strength antibacterial titanium alloy material for additive manufacturing, a preparation method and an application thereof. The high-strength antibacterial titanium alloy material for additive manufacturing comprises the following elemental components by mass percentage: Mo: 8.51-15.45%; Zr: 4.2-8.2%; Fe: 1.1-6.2%; Cu: 2.0-6.1%; the remainder is Ti and unavoidable impurities; among the impurities, C≤0.08%; N≤0.05%; H≤0.015%; and O≤0.20%. By adding and strictly controlling the proportion of Cu element content, this material effectively reduces the elastic modulus of titanium alloy materials, has high hardness, few impurities, high alloy purity, and the oxygen content can be controlled below 1000ppm. It has good weldability and formability, and excellent biocompatibility. It not only enhances the material's ability to resist bacterial infection, but also promotes biological activity, transforming traditional titanium alloys from biologically inert materials to bioactive materials. As a medical material, it is suitable for a variety of additive manufacturing technologies such as laser selective melting and selective laser sintering, expanding the scope of material use in the field of additive manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal materials, and in particular to a high-strength antibacterial titanium alloy material for additive manufacturing, and a preparation method and application thereof. Background Art

[0002] Titanium (Ti) is one of the most widely used oral medical metal materials. However, the elastic modulus of traditional titanium and titanium alloys (about 110GPa) is much higher than that of human bone (about 30GPa). Due to the high elastic modulus, stress shielding is often generated, which shields the shear force / compressive stress that should be applied to the surrounding bone tissue, resulting in insufficient bearing pressure for the bone tissue to be absorbed and atrophied, which in turn leads to problems such as decreased bone density and bone reduction. In addition, titanium is a biologically inert material and does not have biological activity such as antibacterial. In an open microbial environment (such as the human oral cavity and bone defect sites), it often causes infection due to adhesion of bacteria, such as peri-implantitis, post-orthodontic enamel demineralization and gingivitis, and post-operative infection after joint replacement surgery. According to the data of the "Practical Manual for the Prevention and Control of Nosocomial Infections" issued by the World Health Organization, there are more than 14 million patients with nosocomial infections every day in the world, of which about 60% are related to implant infections.

[0003] In recent years, copper (Cu) and titanium and titanium alloy composite materials have attracted extensive attention from the research and engineering communities. On the one hand, Cu is a good β-Ti phase stabilizing element in the titanium alloy system, which is conducive to further reducing the elastic modulus; on the other hand, Cu is an essential trace element for the human body, has good biocompatibility, can catalyze the synthesis of hemoglobin, participate in the development of the cardiovascular system, etc. At the same time, Cu alloying forms Cu 2+ Ions have a strong bactericidal effect and can effectively enhance the alloy material's ability to resist bacterial infection.

[0004] Chinese patents CN102212717A "Anti-infection medical titanium alloy containing copper and its preparation method" and CN102936670A "Anti-infection medical titanium alloy" both mention that adding a certain amount of Cu element to titanium alloy can promote biological activity and enhance antibacterial properties, but the above patents do not consider the effect of the addition of Cu element on different types of titanium alloys, especially the effect on their mechanical properties; while in patents such as CN102943190A "Anti-infection medical titanium alloy" and CN108454190A "Anti-bacterial titanium alloy composite plate and its preparation method", preparation methods of Cu-containing antibacterial titanium alloys are given, but without exception, they need to undergo multi-step pre-treatment such as hot rolling, forging or vacuum hot pressing, and then multiple heat treatments before machining to obtain the material. Not only are the steps cumbersome, but there is also obvious element segregation in the material, and the prepared antibacterial titanium alloy has low structural uniformity and poor stability.

[0005] Compared with traditional manufacturing or machining technology, additive manufacturing technology can rapidly shape a variety of metal materials with different melting points. The molding process does not require auxiliary work such as molds and tools, and can form alloy materials with complex shapes and excellent comprehensive mechanical properties in one go. The formed material has a rapidly solidified non-equilibrium structure with no macro-segregation and dense components, and excellent comprehensive mechanical properties.

[0006] Chinese patent CN115301940B "A Ti-Zr-Cu titanium alloy powder for laser additive manufacturing, its preparation method and application" discloses a Ti-Zr-Cu titanium alloy powder for laser additive manufacturing, but the Cu content of the Ti-Zr-Cu titanium alloy powder is too high, which will have a certain inhibitory effect on cells, resulting in poor biocompatibility of the alloy material obtained from the titanium alloy powder.

[0007] Therefore, it is of great significance to develop a high-strength antibacterial titanium alloy material for additive manufacturing with low modulus, antibacterial and high biocompatibility suitable for 3D printing and its preparation method. Summary of the invention

[0008] In view of the problems of existing titanium alloy medical materials such as too high elastic modulus, complex preparation and poor biocompatibility, the present invention provides a high-strength antibacterial titanium alloy material for additive manufacturing, which is suitable for various additive manufacturing technologies such as laser selective melting and selective laser sintering, has an appropriate elastic modulus, high biocompatibility, can promote biological activity, and has excellent antibacterial properties.

[0009] To achieve the above object, the technical solution adopted by the present invention is:

[0010] A high-strength antibacterial titanium alloy material for additive manufacturing, comprising the following elemental components by mass percentage:

[0011] Mo: 8.51-15.45%; Zr: 4.2-8.2%; Fe: 1.1-6.2%; Cu: 2.0-6.1%; the balance is Ti and unavoidable impurities;

[0012] The impurities include C≤0.08%, N≤0.05%, H≤0.015%, and O≤0.20%.

[0013] Another object of the present invention is to provide a method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing.

[0014] A method for preparing the above-mentioned high-strength antibacterial titanium alloy material for additive manufacturing comprises the following steps:

[0015] S1. Weigh high-purity ingots of ZrFe, MoFe and Ti according to mass percentage, smelt, cool and forge to obtain rods;

[0016] S2. The rod obtained in S1 is vacuum atomized and powdered, and the atomization and powder blowing pressure is 0.3 to 1.2 MPa to obtain Ti-Mo-Zr-Fe alloy powder;

[0017] S3. The Ti-Mo-Zr-Fe alloy powder obtained in S2 and the pure copper powder are ball-milled and mixed, and vacuum dried to obtain Ti-Mo-Zr-Fe-xCu powder, that is, the high-strength antibacterial titanium alloy material for additive manufacturing.

[0018] Furthermore, the purity of the high-purity ingots of ZrFe, MoFe and Ti described in S1 is ≥99.90wt.%.

[0019] Furthermore, the purity of the pure copper powder in S3 is ≥ 99.90wt.%.

[0020] Furthermore, the vacuum gas atomization in S2 is carried out under argon protection at a temperature of 1800-2000°C.

[0021] Furthermore, the particle size of the Ti-Mo-Zr-Fe alloy powder in S3 is 35 to 65 μm, and the particle size of the pure copper powder is 200 nm to 10 μm.

[0022] Furthermore, the ball milling mixing in S3 is carried out under argon protection for 1 to 2 hours, with a rotation speed of 150 to 250 r / min and a ball-to-material mass ratio of (3 to 5):1.

[0023] Furthermore, the vacuum drying temperature in S3 is 80 to 150° C., and the pressure is -0.8 to 0.1 bar.

[0024] Another object of the present invention is to provide an application of a high-strength antibacterial titanium alloy material for additive manufacturing.

[0025] A high-strength antibacterial titanium alloy material for additive manufacturing as described in any of the above items, used for laser 3D printing.

[0026] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0027] (1) The high-strength antibacterial titanium alloy material for additive manufacturing of the present invention greatly reduces the elastic modulus of the titanium alloy by adding Cu. Strictly controlling the content ratio of the Cu element greatly promotes the proliferation and differentiation of MC3T3-E1 osteoblast precursor cells, transforming the traditional titanium alloy from a biologically inert material to a biologically active material. On the other hand, it also promotes the antibacterial effect of the Ti-Mo-Zr-Fe-xCu alloy material on Staphylococcus aureus to varying degrees, making the high-strength antibacterial titanium alloy material for additive manufacturing of the present invention have high biocompatibility, can promote biological activity, and have excellent antibacterial properties.

[0028] (2) The high-strength antibacterial titanium alloy material for additive manufacturing of the present invention is first smelted with an intermediate alloy with a similar melting point to form the required rod material, and then vacuum gas atomization is used to prepare Ti-Mo-Zr-Fe powder, which is then ball-milled and mixed with pure Cu particles to obtain Ti-Mo-Zr-Fe-xCu powder, thereby controlling the uniform melting of elements and reducing the impact of element segregation. The obtained powder has good sphericity, high stability, few satellite balls, and a uniform particle size distribution range. The Ti-Mo-Zr-Fe-xCu alloy material obtained by 3D printing of Ti-Mo-Zr-Fe-xCu powder is mainly composed of equiaxed crystals, and the physical phases are mainly β-Ti and Ti-Cu phases, which improves the hardness of the alloy material, has few impurities, high alloy purity, and the oxygen content can be controlled below 1000ppm, and has good weldability and formability.

[0029] (3) The high-strength antibacterial titanium alloy material for additive manufacturing of the present invention utilizes the advantages of additive manufacturing to process a specific proportion of mixed materials, giving traditional titanium-based materials antibacterial properties, having an appropriate elastic modulus, high biocompatibility, being able to promote biological activity, and having excellent antibacterial properties. It is suitable for a variety of additive manufacturing technologies such as laser selective melting and selective laser sintering, expanding the scope of material use in the field of additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0031] Figure 1 This is a microstructure morphology of a sample obtained by additive manufacturing of a high-strength antibacterial titanium alloy material for additive manufacturing in Example 1.

[0032] Figure 2 This is the microstructure morphology of the Ti-Mo-Zr-Fe alloy powder prepared in Comparative Example 5.

[0033] Figure 3 This is the microstructure morphology of the Ti-Mo-Zr-Fe alloy powder prepared in Comparative Example 6.

[0034] Figure 4 This is the microstructure morphology of the high-strength antibacterial titanium alloy material for additive manufacturing prepared in Comparative Example 7.

[0035] Figure 5 This is a CT morphology image of the porous structure manufactured in the present invention taken out from a rat 12 weeks after being implanted. DETAILED DESCRIPTION

[0036] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention is further described by the following examples. Obviously, the following examples are only part of the embodiments of the present invention, rather than all the embodiments; it should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.

[0037] The raw materials in the examples can all be obtained commercially; unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0038] Example 1

[0039] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing comprises the following steps:

[0040] S1. Weigh high-purity ingots of ZrFe (Zr content is 90wt.%, the balance is Fe and inevitable impurities), MoFe (Mo content is about 85wt.%, the balance is Fe and inevitable impurities) and Ti (Mo:Zr:Fe:Ti=11.38:6.20:1.80:80.52) with a purity of ≥99.90wt.% according to mass percentage, put them into an electroslag furnace for smelting, cooling and forging to obtain a rod with a diameter of 50mm, a length of 700mm and a front end with a cone angle of 90 degrees;

[0041] S2. The rod obtained in S1 was powdered by electrode induction melting vacuum gas atomization without a crucible and under the protection of high-purity argon (99.999 vol.%), the feed rate was set to 200 mm / min, the speed was adjusted to 20 r / min, the temperature was 1900 ° C, high-pressure (supersonic) high-purity argon (99.999 vol.%) was selected as the powder blowing gas, and the atomization powder blowing pressure was 1.0 MPa to obtain Ti-Mo-Zr-Fe alloy powder;

[0042] S3. The spherical Ti-Mo-Zr-Fe alloy powder with a particle size distribution of 15 to 53 μm and a purity of ≥99.90 wt.% and a particle size of 500 nm obtained in S2 (Ti-Mo-Zr-Fe:Cu=97.88:2.12) are placed in a planetary ball mill in proportion for ball milling and mixing. In addition to filling the ball mill tank with 1 / 2 of the tank volume of anhydrous ethanol (purity 99%) as the liquid medium, the remaining tank volume of 1 / 2 is filled with high-purity argon (99.999 vol.%), the powder mixing time is 1.5 hours, the rotation speed is 200r / min, the ball-to-material mass ratio is 3:1, vacuum drying, vacuum pressure = -0.1bar, insulation temperature = 100°C, heating rate = 80°C / min, insulation time 2h, and then reduced to 25°C to obtain Ti-Mo-Zr-Fe-xCu powder, put it into a vacuum bag and store it in a vacuum to obtain the high-strength antibacterial titanium alloy material for additive manufacturing.

[0043] Example 2

[0044] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing comprises the following steps:

[0045] S1. Weigh high-purity ingots of ZrFe (Zr content is 90wt.%, the balance is Fe and inevitable impurities), MoFe (Mo content is about 85wt.%, the balance is Fe and inevitable impurities) and Ti (Mo:Zr:Fe:Ti=11.38:6.20:1.80:80.52) with a purity of ≥99.90wt.% according to mass percentage, put them into an electroslag furnace for smelting, cooling and forging to obtain a rod with a diameter of 50mm, a length of 700mm and a front end with a cone angle of 90 degrees;

[0046] S2. The rod obtained in S1 was powdered by electrode induction melting vacuum gas atomization without a crucible and under the protection of high-purity argon (99.999 vol.%), the feed rate was set to 200 mm / min, the speed was adjusted to 20 r / min, the temperature was 1900 ° C, high-pressure (supersonic) high-purity argon (99.999 vol.%) was selected as the powder blowing gas, and the atomization powder blowing pressure was 1.0 MPa to obtain Ti-Mo-Zr-Fe alloy powder;

[0047] S3. The spherical Ti-Mo-Zr-Fe alloy powder with a particle size distribution of 15 to 53 μm and a purity of ≥99.90 wt.% and a particle size of 500 nm obtained in S2 (Ti-Mo-Zr-Fe:Cu=95.69:4.31) are placed in a planetary ball mill in proportion for ball milling and mixing. In addition to filling the ball mill tank with 1 / 2 of the tank volume with anhydrous ethanol (purity 99%) as the liquid medium, the remaining tank volume is 1 / 2 of the tank volume. / 2 is filled with high-purity argon (99.999 vol.%), the powder mixing time is 1.5 hours, the rotation speed is 200r / min, the ball-to-material mass ratio is 3:1, vacuum drying, vacuum pressure = -0.1bar, insulation temperature = 100°C, heating rate = 80°C / min, insulation time 2h, and then reduced to 25°C to obtain Ti-Mo-Zr-Fe-xCu powder, put it into a vacuum bag and store it in a vacuum to obtain the high-strength antibacterial titanium alloy material for additive manufacturing.

[0048] Example 3

[0049] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing comprises the following steps:

[0050] S1. Weigh high-purity ingots of ZrFe (Zr content is 90wt.%, the balance is Fe and inevitable impurities), MoFe (Mo content is about 85wt.%, the balance is Fe and inevitable impurities) and Ti (Mo:Zr:Fe:Ti=11.38:6.20:1.80:80.52) with a purity of ≥99.90wt.% according to mass percentage, put them into an electroslag furnace for smelting, cooling and forging to obtain a rod with a diameter of 50mm, a length of 700mm and a front end with a cone angle of 90 degrees;

[0051] S2. The rod obtained in S1 was powdered by electrode induction melting vacuum gas atomization without a crucible and under the protection of high-purity argon (99.999 vol.%), the feed rate was set to 200 mm / min, the speed was adjusted to 20 r / min, the temperature was 1900 ° C, high-pressure (supersonic) high-purity argon (99.999 vol.%) was selected as the powder blowing gas, and the atomization powder blowing pressure was 1.0 MPa to obtain Ti-Mo-Zr-Fe alloy powder;

[0052] S3. The spherical Ti-Mo-Zr-Fe alloy powder with a particle size distribution of 15 to 53 μm and a purity of ≥99.90 wt.% and a particle size of 500 nm obtained in S2 (Ti-Mo-Zr-Fe:Cu=93.95:6.05) are placed in a planetary ball mill in proportion for ball milling and mixing. In addition to filling the ball mill tank with 1 / 2 of the tank volume of anhydrous ethanol (purity 99%) as the liquid medium, the remaining tank volume of 1 / 2 is filled with high-purity argon (99.999 vol.%), the powder mixing time is 1.5 hours, the rotation speed is 200r / min, the ball-to-material mass ratio is 3:1, vacuum drying, vacuum pressure = -0.1bar, insulation temperature = 100°C, heating rate = 80°C / min, insulation time 2h, and then reduced to 25°C to obtain Ti-Mo-Zr-Fe-xCu powder, put it into a vacuum bag and store it in a vacuum to obtain the high-strength antibacterial titanium alloy material for additive manufacturing.

[0053] Comparative Example 1

[0054] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 1, except that: compared with Example 1, this comparative example lacks copper element.

[0055] Comparative Example 2

[0056] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 1, except that: compared with Example 1, the copper content in this comparative example is 1wt.%.

[0057] Comparative Example 3

[0058] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 1, except that: compared with Example 1, the copper content in this comparative example is 7wt.%.

[0059] Comparative Example 4

[0060] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing comprises the following steps:

[0061] S1. Weigh high-purity ingots of Zr, Fe, Mo, Ti and Cu with a purity of ≥99.90wt.% according to mass percentage, put them into an electroslag furnace for smelting, cooling and forging to obtain a rod with a diameter of 50mm, a length of 700mm and a front end with a cone angle of 90 degrees;

[0062] S2. The rod obtained in S1 is powdered by electrode induction melting and vacuum gas atomization without a crucible and under the protection of high-purity argon (99.999 vol.%). The feed rate is set to 200 mm / min, the rotation speed is adjusted to 20 r / min, the temperature is 1900°C, and high-pressure (supersonic) high-purity argon (99.999 vol.%) is selected as the powder blowing gas. The atomization powder blowing pressure is 1.0 MPa to obtain Ti-Mo-Zr-Fe-xCu alloy powder.

[0063] Comparative Example 5

[0064] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 1, except that: compared with Example 1, the atomization powder blowing pressure of Comparative Example S2 is 0.2 MPa.

[0065] Comparative Example 6

[0066] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 1, except that: compared with Example 1, the atomization powder blowing pressure of this comparative example S2 is 1.3 MPa.

[0067] Comparative Example 7

[0068] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 1, except that: compared with Example 1, the particle size of the spherical pure copper powder S3 in this comparative example is 11 to 73 μm.

[0069] Comparative Example 8

[0070] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 2, except that: compared with Example 2, the particle size of the spherical pure copper powder in this comparative example S3 is 11 to 73 μm.

[0071] Comparative Example 9

[0072] A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, wherein the steps not specifically described are the same as those in Example 3, except that: compared with Example 3, the particle size of the spherical pure copper powder in this comparative example S3 is 11 to 73 μm.

[0073] The specific element contents and parameters of Examples 1 to 3 and Comparative Examples 1 to 9 are shown in Table 1.

[0074] Table 1 Element contents and parameter settings of Examples 1 to 3 and Comparative Examples 1 to 9

[0075]

[0076] Solidworks 3D modeling software was used to establish a 3D model of the alloy material, which was then imported into Magics software for parts placement and laser scanning sequence setting. The Ti-Mo-Zr-Fe-xCu powder obtained in Examples 1 to 3 and Comparative Examples 1 to 9 was poured into a powder storage bin of a laser selective melting additive manufacturing system, and the EOS M290 system produced by EOS GmbH of Germany was used for manufacturing by SLM (Selective Laser Melting) technology. The laser spot was 100 μm, the laser power was 100 W, the layer thickness was 30 μm, the scanning spacing was 90 μm, the scanning speed was 550 mm / s, and a zigzag scanning method was used to obtain a test sample.

[0077] Among them, since the powder stability of Comparative Example 4 is extremely poor, the irregular powder blown out of Comparative Example 5 is relatively large, and the powder satellite balls blown out of Comparative Example 6 are extremely large and irregular, they are not suitable for laser 3D printing, and test samples cannot be obtained, so they are tested in powder form.

[0078] The above samples were subjected to performance tests, and the specific test process is as follows:

[0079] (1) Microstructure test

[0080] Figure 1 This is the microstructure morphology of Ti-Mo-Zr-Fe-xCu after the powder prepared in Example 1 was formed by SLM. The grain structure is fine, there is no Cu particle enrichment or segregation, and the SLM melt path is fine, and its solidification process is not affected by the addition of Cu particles.

[0081] The characterization test results of the remaining embodiments are basically consistent with those of Embodiment 1.

[0082] Comparative Example 4 is directly prepared using high-purity ingots of Zr, Fe, Mo, Ti and Cu. Since the melting point of Mo is relatively high (about 2623 degrees), but the boiling point of Fe is about 2750 degrees, and the boiling point of Cu is about 2567 degrees, the melting temperature must be accurately maintained to ensure that the Fe and Cu elements do not evaporate, resulting in local segregation caused by the failure of some Mo to melt in the prepared rod. Moreover, since the density of Mo is much greater than that of Ti, and the density of Cu is close to twice that of Ti, its composition will show obvious segregation when sampling at different parts of the rod. The average composition of Mo at the head, middle and tail of the material is approximately 7.85wt.%, 9.12wt.% and 11.23wt.%, respectively. The average composition of Cu also has a large deviation, and the stability and consistency of the powder are extremely poor, and laser 3D printing cannot be performed.

[0083] In comparative example 5, the powder blowing pressure in step S2 is set to 0.2 MPa, and the other parameters remain unchanged. Due to the low powder blowing pressure, more irregular powder is blown out, such as Figure 2 As shown, the yield of powder suitable for 3D printing in the particle size range of 15 to 75 μm is low.

[0084] In comparative example 6, the powder blowing pressure in step S2 is set to 1.3 MPa, and the other parameters remain unchanged. Due to the excessively high powder blowing pressure, the powder satellites blown out are extremely numerous and irregular, such as Figure 3 As shown, it is not suitable for use in laser 3D printing.

[0085] In comparative examples 7 to 9, the Cu particles in step S4 are selected to be 10-73 μm, and the other parameters remain unchanged. Although the sphericity after mixing is not affected, due to the small difference in particle size between the two, there are more unmelted Cu particles and a large number of holes in the microstructure after 3D printing, such as Figure 4 As shown, unmelted Cu particles can be clearly observed in the microstructure of the Ti-Mo-Zr-Fe-xCu powder prepared in Comparative Example 6 after 3D printing, resulting in a sharp decrease in the mechanical properties after printing, and the powder is not suitable for use in medical devices with large load-bearing parts.

[0086] (2) Mechanical properties test

[0087] The samples prepared in Examples 1 to 3 and Comparative Examples 1 and 7 to 9 were subjected to stress-strain performance tests during stretching at room temperature (25°C). The test method was as follows: a tensile test was conducted at a displacement rate of 1 mm / min at room temperature according to ASTM E8M standard. Mechanical properties including tensile strength (UTS), yield strength (YS) and fracture strain were directly read from the INSTRON tensile tester, and strain failure was evaluated by a 10 mm range strain gauge and an electronic extensometer installed on the gauge portion of the test sample. The elastic modulus was calculated based on the stress-strain curve. For each experimental group, three samples were tested and the average value was calculated.

[0088] The samples prepared in Examples 1 to 3 and Comparative Examples 1 and 7 to 9 were subjected to an average microhardness test. The test method was as follows: a microhardness tester (model: Leitz Wetzlar, Germany) was used to measure the Vickers microhardness of the sample. The load used was 200 g and the loading time was 25 s. The surface roughness of the SLM sample test surface was polished to less than 0.15 μm, and the microhardness values ​​at different positions on the SLM sample surface were measured. The average value was taken after 10 measurements. The test results are shown in Table 2.

[0089] Table 2 Mechanical properties of Examples 1 to 3 and Comparative Examples 1 and 6 to 8

[0090]

[0091]

[0092] It can be seen from Table 2 that the high-strength antibacterial titanium alloy materials for additive manufacturing of Examples 1-3 of the present invention all have excellent hardness and low elastic modulus. Although the mechanical properties decrease to a certain extent with the increase of the copper content, the comprehensive mechanical properties are excellent and suitable for use in high-end biomedical equipment and the like; while in Comparative Example 1, no copper element is added, and the elastic modulus reaches 88.7 GPa. The pure copper powder used in Comparative Examples 6 to 8 has a large particle size, and a large amount of hard particles such as Ti-Cu are generated, which causes its elongation after fracture to drop sharply, and the elastic modulus of the prepared samples also reaches more than 70 GPa, which is not suitable for medical materials.

[0093] (3) Biological performance test

[0094] The samples prepared in Examples 1-3 and Comparative Examples 1-3 were tested for in vitro cytotoxicity, proliferation and differentiation.

[0095] The analysis was performed using MC3T3-E1 osteoblast precursor cells in accordance with the international standard ISO 10993-5. Before use in the cytotoxicity assay, liquid extracts of the samples were prepared (37°C, 10% FBS (v / v), 3 cm in α-MEM 2 / mL) and sterilized by filtration, and the cytotoxicity was evaluated using a cell counting kit-8 (CCK-8). BMSCs were plated at 1×10 4 The density of cells was seeded in 96-well plates (Nest, USA) for one day, and then the medium was replaced with liquid extracts of medical grade polyethylene (negative control, non-cytotoxic), α-MEM (positive control, providing reproducible cytotoxicity) containing 10% FBS (v / v) and 10% dimethyl sulfoxide (DMSO) and the liquid extracts of the SLM Ti-Mo-Zr-Fe-xCu samples from each group (100 μL / well) for 1 day, 3 days, 5 days and 7 days. Subsequently, 10 μL of CCK-8 solution was added to each well of the plate, and the plate was incubated for two hours under light. The absorbance at 450 nm was measured. The values ​​of the negative control wells were averaged and used as 100% cell viability. All other values ​​were then averaged relative to their groups and compared with the negative control group.

[0096] Anti-Staphylococcus aureus test was performed as follows:

[0097] LB liquid culture medium: Use a measuring cylinder to measure 100 mL of distilled water and pour it into a 250 mL reagent bottle. Use an analytical electronic balance to weigh 2.5 g of LB broth culture medium and add it to mix well. Sterilize it in a high-temperature and high-pressure steam sterilizer at 121°C for 15 minutes and set aside for use.

[0098] LB solid culture medium - use a measuring cylinder to measure 100mL of distilled water and pour it into a 250mL reagent bottle. Use an analytical electronic balance to weigh 2.5g of LB broth culture medium and 1.5g of agar powder respectively. Add the above weighed reagents and mix well. Sterilize in a high-temperature and high-pressure steam sterilizer at 121℃ for 15min. When the culture medium cools to about 40-50℃, use an electric pipette to draw 15mL of culture medium and pour it into a disposable sterile plate.

[0099] Take two 12mL bacterial culture tubes, add 3mL LB liquid medium to each, pick a single colony from the solid culture medium of Staphylococcus aureus and add it to the liquid culture medium, and use the other tube as a blank control. Place in a constant temperature shaker (37℃, 200rpm) and shake culture overnight (15h).

[0100] Wipe the surface of the sample with 75% alcohol cotton, and after drying, place it in a disposable culture dish with the corresponding number, sterilize it with ultraviolet light on both sides for 30 minutes, and set aside.

[0101] Dilute Staphylococcus aureus to 106 CFU / mL with LB liquid medium. Add 50 μL of diluted bacterial solution to the sample surface, and do not add sample to the control group. Cover with a cover film and press gently. Place in a constant temperature incubator at 37°C and culture for 18 hours.

[0102] After the culture is completed, rinse with 2 mL of sterile PBS, and dilute it 10 times with PBS solution, and evenly spread 100 μL of the dilution on the LB solid medium. Incubate it in a 37°C constant temperature incubator for 18 hours, take it out, take pictures and record the number of colonies. Then count the colonies and calculate the antibacterial rate according to GB4789.2-2016.

[0103] The specific test results of each embodiment and comparative example are shown in Table 3.

[0104] Table 3 Biological properties of Examples 1 to 3 and Comparative Examples 1 to 3

[0105]

[0106]

[0107] It can be judged from Table 3 that the high-strength antibacterial titanium alloy materials for additive manufacturing of Examples 1-3 of the present invention are not only non-cytotoxic, but also show excellent antibacterial and osteogenic effects. Not only does the bactericidal effect significantly improve with the continuous increase of the Cu element, but it also has a positive effect on the differentiation and proliferation of MC3T3-E1 osteoblasts; while Comparative Example 1 does not add copper and does not have antibacterial properties. The copper content of Comparative Example 2 is 1.0wt.%, the antibacterial rate is low and has no obvious effect on promoting the growth of MC3T3 cells. The copper content of Comparative Example 3 is 7.0wt.%, and the antibacterial rate is 99.5%, but the survival rate of MC3T3 cells is greatly reduced to 25.2%, which indicates that the increase of the Cu element has a great inhibitory effect on the growth of the cell membrane, resulting in poor biocompatibility.

[0108] Figure 5 The Ti-Mo-Zr-Fe-xCu porous structure material developed using this patent did not show any abnormality after being implanted in rats for 3 months. After the Ti-Mo-Zr-Fe-xCu porous structure was implanted in rats for 12 weeks and removed for CT testing, it was found that there was obvious new bone ingrowth (as shown in the dark part), showing excellent bone integration, indicating that the personalized SLM Ti-Mo-Zr-Fe-xCu alloy with excellent comprehensive mechanical properties and biological activity developed within the appropriate range of Cu content has excellent potential for product development and good application prospects.

[0109] In summary, the high-strength antibacterial titanium alloy material for additive manufacturing of the present invention effectively reduces the elastic modulus of the titanium alloy material by adding and strictly controlling the proportion of the Cu element content. It has high hardness, few impurities, high alloy purity, and the oxygen content can be controlled below 1000ppm. It has good weldability and formability, and at the same time has excellent biocompatibility. It not only enhances the material's ability to resist bacterial infection, but also promotes biological activity, transforming traditional titanium alloys from biologically inert materials into bioactive materials. As a medical material, it is suitable for various additive manufacturing technologies such as laser selective melting and selective laser sintering, expanding the scope of material use in the field of additive manufacturing.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing, characterized in that: The following steps are involved: S1. Weigh high-purity ingots of ZrFe, MoFe and Ti according to mass percentage, smelt, cool and forge to obtain rods; S2. The rod obtained in S1 is vacuum atomized and powdered, and the atomization and powder blowing pressure is 0.3~1.2MPa to obtain Ti-Mo-Zr-Fe alloy powder; S3. The Ti-Mo-Zr-Fe alloy powder and pure copper powder obtained in S2 are ball-milled and mixed, and vacuum dried to obtain Ti-Mo-Zr-Fe-xCu powder, that is, the high-strength antibacterial titanium alloy material for additive manufacturing; The particle size of the Ti-Mo-Zr-Fe alloy powder in S3 is 35-65µm, and the particle size of the pure copper powder is 200nm-10μm; The high-strength antibacterial titanium alloy material for additive manufacturing includes the following elemental components by mass percentage: Mo: 8.51~15.45%; Zr: 4.2~8.2%; Fe: 1.1~6.2%; Cu: 2.0~6.1%; the balance is Ti and unavoidable impurities; Among the impurities, C≤0.08%; N≤0.05%; H≤0.015%; O≤0.20%.

2. The method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing according to claim 1, characterized in that: The purity of the high-purity ingots of ZrFe, MoFe and Ti described in S1 is ≥99.90wt.%.

3. The method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing according to claim 1, characterized in that: The purity of the pure copper powder in S3 is ≥99.90wt.%.

4. The method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing according to claim 1, characterized in that: The vacuum gas atomization in S2 is carried out under the protection of argon gas at a temperature of 1800-2000°C.

5. The method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing according to claim 1, characterized in that: The ball milling mixing in S3 is carried out under argon protection for 1 to 2 hours at a rotation speed of 150 to 250 r / min, and the ball-to-material mass ratio is (3 to 5):

1.

6. The method for preparing a high-strength antibacterial titanium alloy material for additive manufacturing according to claim 1, characterized in that: The vacuum drying temperature in S3 is 80-150° C. and the pressure is -0.8-0.1 bar.