An evaporator with non-uniform pore structure inside and outside and a method for preparing the same

By applying photothermal conversion substances and hydrophilic polymer materials on the surface of the sponge, an internal and external non-uniform pore structure evaporator is formed, which solves the problems of evaporation rate and salt resistance under high salt concentration in traditional three-dimensional interface evaporators, and achieves high efficiency Seawater desalination and heavy metal wastewater treatment.

CN118005122BActive Publication Date: 2024-12-03CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410285330.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-12-03
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

Traditional three-dimensional interface evaporators are difficult to increase the evaporation rate under high salt concentration conditions and have poor salt resistance, resulting in salt crystallization and affecting evaporation performance and durability.

Method used

Design an internal and external non-uniform pore structure evaporator, and regulate water transport by applying photothermal conversion substances and hydrophilic polymer materials on the surface of high-porosity sponges. Transport and heat localization to improve the return rate of salt ions and thermal insulation performance.

Benefits of technology

It achieves high evaporation rate and excellent salt resistance performance, reduces the heat loss of the evaporator, is suitable for remote areas without high energy drive, and is suitable for seawater desalination and heavy metal wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118005122B_ABST
    Figure CN118005122B_ABST
Patent Text Reader

Abstract

The present invention discloses an evaporator with an internal and external non-uniform pore structure, which belongs to the field of seawater desalination and aims to synergistically enhance the evaporation efficiency and salt resistance performance of the evaporator under high salt concentration conditions. The outer layer of the evaporator with an internal and external non-uniform pore structure is a low-porosity interface evaporation layer, and the internal body is a high-porosity porous structure; the low-porosity interface evaporation layer is mainly composed of a gel structure and a photothermal conversion material attached to the gel structure, wherein the gel structure is formed by cross-linking a hydrophilic polymer material. The high-porosity porous structure is mainly composed of a high-porosity sponge. The present invention realizes precise control of the water transport process through the internal and external non-uniform design of the pore structure, which greatly reduces the heat conduction loss of the evaporator while accelerating the salt ion reflux rate, effectively coordinating the contradiction between water transport and heat localization, thereby realizing the organic unity of efficient evaporation and efficient salt resistance of the evaporator.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solar-driven seawater desalination, and in particular to an evaporator with internal and external non-uniform pore structures. Background Art

[0002] With the rapid increase of population and the aggravation of environmental pollution, the shortage of fresh water resources is becoming increasingly serious, and the search for fresh water resources is imminent. The earth has a huge amount of seawater reserves, and solar energy is clean and sustainable. Using solar energy for seawater desalination is an ideal way to solve the shortage of fresh water. Due to its high evaporation rate, clean and pollution-free, and low cost, solar-driven interfacial evaporation technology has shown broad application prospects in heavy metal wastewater purification and seawater desalination, and has attracted widespread attention from scholars. The interfacial evaporation structure has been continuously developed from a two-dimensional interface evaporation structure to a three-dimensional interface evaporation structure, and the evaporation rate has been continuously increasing. However, the pores inside and outside the traditional three-dimensional structure interface evaporator are consistent, and the salt water is transported from the bottom of the lower end to the evaporation interface as a whole. The pore distribution inside the evaporator is staggered, the water supply path is long, and the salt ion reflux is slow, resulting in poor salt resistance of the three-dimensional structure interface evaporator. It is easy to form salt crystals at the evaporation interface, which will seriously affect the evaporation performance and durability of the evaporator. Although the salt resistance of the evaporator can be improved by preparing some through holes, the heat loss from the evaporator to the bulk water will increase, reducing the evaporation rate. The three-dimensional interface evaporator is difficult to further improve the evaporation rate under high salt concentration conditions due to its longitudinal overall water transport, which restricts the development and practical application of solar desalination. Therefore, it is very necessary to design an evaporator that can effectively coordinate water transport and heat localization to achieve high evaporation and salt resistance. Summary of the invention

[0003] The purpose of the present invention is to provide an evaporator with an internal and external non-uniform pore structure that can accurately regulate water transport, effectively reduce the heat conduction loss of the evaporator, accelerate the salt ion reflux rate, coordinate the contradiction between water transport and heat localization, and achieve effective unification of high evaporation and salt resistance performance.

[0004] To achieve the above object, the preparation method adopted by the present invention is:

[0005] 1) Ultrasonic mixing the photothermal conversion material and the dispersant at a mass ratio of 1:100 to 1:200 to obtain a low-concentration photothermal conversion material solution;

[0006] 2) coating a low-concentration photothermal conversion substance solution on the surface of a high-porosity sponge with a porosity of 90-99% and an internal pore size distribution of 100-300 μm, and then placing it in a constant temperature drying oven for drying to obtain a high-porosity sponge with a photothermal conversion substance coated on the surface;

[0007] 3) mixing a hydrophilic polymer material and water at a mass ratio of 1:15-30 to form a hydrophilic polymer solution, and then adding a cross-linking agent glutaraldehyde and a hydrophilic polymer material to the hydrophilic polymer solution at a ratio of 1:7-15 to prepare a hydrophilic polymer material mixed aqueous solution;

[0008] 4) Applying a mixed aqueous solution of a hydrophilic polymer material on the outer surface of a high-porosity sponge coated with a photothermal conversion substance, and placing the sponge in a constant temperature drying oven to dry after the cross-linking reaction to obtain a cross-linked sample;

[0009] 5) Ultrasonic mixing the photothermal conversion material and the dispersant at a mass ratio of 1:20 to 1:50 to obtain a high-concentration photothermal conversion material solution;

[0010] 6) Applying a high-concentration photothermal conversion material solution on the cross-linked sample surface, and then drying it in a constant temperature drying oven, to obtain an internal and external non-uniform pore structure evaporator having a low-porosity interface evaporation layer outside the high-porosity sponge surface.

[0011] The photothermal conversion material is one or more of carbon black, carbon dots, graphene, and polydopamine.

[0012] The dispersant is one or more of ethanol, isopropanol and n-butanol.

[0013] The high-porosity sponge is melamine sponge, polyvinyl alcohol sponge, melamine sponge or polyurethane sponge.

[0014] The constant temperature drying temperature is 60-80° C., and the constant temperature drying time is 8-12 hours.

[0015] The hydrophilic polymer material is one or more of polyvinyl alcohol, chitosan, acrylamide, acrylic acid and their derivatives.

[0016] The evaporator with internal and external non-uniform pore structure made by the above preparation method comprises a main body with an internal high-porosity structure and an outer low-porosity interface evaporation layer, wherein the porosity of the main body with an internal high-porosity structure is 90-99%, and the internal pore size distribution is 100-300 μm, and the porosity of the outer low-porosity interface evaporation layer is 70-90%, the pore size distribution is 200 nm-50 μm, and the thickness is 0.1-1 mm.

[0017] The main body of the internal high-porosity structure is a high-porosity melamine sponge, a polyvinyl alcohol sponge, a melamine sponge or a polyurethane sponge.

[0018] The outer low-porosity interface evaporation layer is composed of a gel structure formed by cross-linking of hydrophilic polymer materials and a photothermal conversion substance attached to the gel structure;

[0019] The hydrophilic polymer material is one or more of chitosan, polyvinyl alcohol, acrylamide, acrylic acid and their derivatives;

[0020] The photothermal conversion material is one or more of carbon black, carbon dots, graphene, and polydopamine.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The evaporator with non-uniform internal and external pore structure prepared by the present invention has low material cost and simple preparation method and can be mass-produced.

[0023] 2. Compared with the current seawater desalination technology mainly based on reverse osmosis membrane method and distillation method, the only energy source of this invention is the sun, which does not need to consume high-grade energy to drive. Therefore, it does not need to rely on mature infrastructure and industrial production technology, and is suitable for remote mountainous areas and islands.

[0024] 3. Compared with conventional two-dimensional interface evaporation devices, the present invention can absorb energy from the surrounding environment, thereby increasing the overall evaporation rate.

[0025] 4. Compared with the existing three-dimensional interface evaporation device, the present invention adjusts the porosity inside and outside the evaporator so that the high-porosity structure of the internal body of the evaporator does not bear the responsibility of water transportation. Therefore, the internal body of the evaporator has good thermal insulation performance, which greatly reduces the heat loss of the evaporator. And because the surface water supply path is simple and the water transportation speed is fast, the salt ions can flow back quickly. Based on the above characteristics, the present invention has excellent evaporation and salt resistance performance, and can achieve efficient and stable seawater desalination under natural light and simulated seawater with different salt concentrations. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the evaporation process of the evaporator with non-uniform internal and external pore structure of the present invention.

[0027] Figure 2 This is a SEM electron microscope image of the surface of the evaporator with non-uniform pore structure inside and outside prepared in Example 1 of the present invention.

[0028] Figure 3 This is a diagram of the evaporation performance of the evaporator with non-uniform internal and external pore structures prepared in Example 1 of the present invention and the random pore evaporator prepared in Comparative Example 1.

[0029] Figure 4 These are the evaporation performance diagrams of evaporators with internal and external non-uniform pore structures prepared in Examples 1, 2, 3, and 4 of the present invention.

[0030] Figure 5 This is a test diagram of the salt resistance performance of the evaporator with non-uniform pore structure inside and outside prepared in Example 1 of the present invention.

[0031] Figure 6 Comparison of the treatment of heavy metal wastewater and seawater by the evaporator with non-uniform internal and external pore structure prepared in Example 1 of the present invention before and after.

[0032] Figure 7 This is the structural strength and cycle test of the evaporator with non-uniform pore structure inside and outside prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0033] Embodiment 1:

[0034] Step 1: Select a melamine sponge with a high porosity of 98% and a pore size of 150-250 μm, and cut the melamine sponge into a rectangular structure with a length of 2 cm, a width of 2 cm, and a height of 4 cm;

[0035] Step 2: Prepare a low-concentration carbon black solution by mixing 0.5 g of carbon black with 60 ml of ethanol solution and ultrasonically dispersing for 30 minutes to prepare a low-concentration carbon black solution.

[0036] Step 3: Apply low-concentration carbon black solution evenly on the surface of the rectangular melamine sponge, and then place it in a constant temperature oven at 60°C to dry for 8 hours.

[0037] Step 4: Prepare a mixed solution of polyvinyl alcohol and glutaraldehyde by heating and stirring 2 g of polyvinyl alcohol, 0.25 ml of glutaraldehyde and 60 ml of water to dissolve, thereby preparing a mixed solution of polyvinyl alcohol and glutaraldehyde.

[0038] Step 5: Evenly brush the mixed solution of polyvinyl alcohol and glutaraldehyde on the surface of the rectangular melamine sponge in step 3, and then spray 3wt% diluted hydrochloric acid to make it gel, and then put it into a constant temperature oven at 60°C to dry for 8h to form a gel on the surface of the rectangular melamine sponge.

[0039] Step 6: Prepare a high-concentration carbon black solution by ultrasonically stirring 3 g of carbon black with 60 ml of anhydrous ethanol for 30 minutes.

[0040] Step 7: Evenly brush the high-concentration carbon black solution on the dried gel surface, and then put it into a constant temperature oven at 60°C for 8 hours to obtain an evaporator with non-uniform pore structure inside and outside.

[0041] The evaporator with internal and external non-uniform pore structure comprises a main body with an internal high-porosity structure and an outer low-porosity interface evaporation layer. The main body with an internal high-porosity structure adopts a melamine sponge with a porosity of 98% and a pore size of 150-250 μm. The outer low-porosity interface evaporation layer has a porosity of 70-90%, a pore size distribution of 200 nm-50 μm, and a thickness of 0.1-1 mm.

[0042] Embodiment 2:

[0043] The difference from Example 1 is that the size of the melamine sponge is 2 cm in length, 2 cm in width and 2 cm in height, and the rest of the contents are exactly the same as those in Example 1.

[0044] Embodiment 3:

[0045] The difference from Example 1 is that the size of the melamine sponge is 2 cm in length, 2 cm in width and 6 cm in height, and the rest of the contents are exactly the same as those in Example 1.

[0046] Example 4

[0047] The difference from Example 1 is that the size of the melamine sponge is 2 cm in length, 2 cm in width and 8 cm in height, and the rest of the contents are exactly the same as those in Example 1.

[0048] Comparative Example 1

[0049] The difference from Example 1 is that Example 1 is coated only on the surface, while Comparative Example 1 is overall immersion, so that the porosity inside and outside the evaporator is consistent, and the other materials are consistent.

[0050] Performance test: Figure 2 It can be seen that compared with the blank melamine sponge ( Figure 2 a, d), after loading low concentration of carbon black, carbon black particles are attached to the melamine sponge base skeleton, making the melamine sponge skeleton thicker and the pore size initially reduced ( Figure 2 b, e). Then, the polyvinyl alcohol mixed solution is subjected to gel reaction on the surface layer, and then the carbon black solution is applied to the surface layer, and the surface pore size is further reduced ( Figure 2 c, f).

[0051] The evaporation rate of the evaporator with non-uniform pore structure inside and outside prepared in Example 1 and the uniform pore evaporator prepared in the comparative example were tested. The results are as follows: Figure 3 a. The evaporation rate of the evaporator with non-uniform internal and external pore structure prepared in Example 1 is 4.98 kg·m -2 , which is significantly higher than the evaporation rate of the uniform pore evaporator in Comparative Example 1 of 3.9 kg·m -2 , Figure 3 b is a high light intensity performance test of the evaporator with internal and external non-uniform pore structure prepared in Example 1. It can be seen that the evaporation rate of the evaporator with internal and external non-uniform pore structure increases steadily with the increase of light intensity.

[0052] Figure 4 The evaporation performance diagram of the evaporator with non-uniform pore structure inside and outside prepared for implementation cases 1, 2, 3, and 4 shows that the evaporation rate increases with the increase of the evaporator height. The evaporation rate of the evaporator with non-uniform pore structure inside and outside of Example 4 with a height of 8 cm is 6.0 kg·m -2 .

[0053] Figure 5 The salt resistance performance of the evaporator with non-uniform pore structure inside and outside prepared in Example 1 and the random pore evaporator prepared in Comparative Example 1 was tested. The evaporator with non-uniform pore structure inside and outside was operated stably for 48 hours in 25% nearly saturated salt water, and no salt crystals were found on the surface. Figure 5 b. After the uniform pore evaporator was operated in 25% nearly saturated brine for 48 hours, the entire surface was covered with white salt crystals. Figure 5 a.

[0054] Figure 6 The figure shows a comparison of the treatment of heavy metal wastewater and seawater by the evaporator with internal and external non-uniform pore structure prepared in Example 1. It can be seen from the figure that the concentrations of heavy metal ions and salt ions are significantly reduced after evaporation and condensation by the evaporator with internal and external non-uniform pore structure, and can reach the ion concentration standard of drinking water.

[0055] The reliability test of the evaporator with non-uniform internal and external pore structure in Example 1 was carried out. Figure 7 Figure a is a cyclic stability test. The stability is good after 10 cyclic tests. Figure b is a structural strength test of the evaporator with non-uniform pore structure inside and outside. It can be seen that a 500g weight is placed on the top of the evaporator, and the evaporator has no obvious deformation, and the height is consistent before and after extrusion, and the structural strength is good.

[0056] Embodiment 5:

[0057] 1) Ultrasonic mixing of carbon dots as a photothermal conversion material and isopropanol as a dispersant at a mass ratio of 1:150 to obtain a low-concentration photothermal conversion material solution;

[0058] 2) coating a low-concentration photothermal conversion substance solution on the surface of a high-porosity melamine sponge with a porosity of 90% and an internal pore size distribution of 100 to 300 μm, and then placing the sponge in a constant temperature drying oven at 70° C. for 10 hours to obtain a high-porosity sponge with a photothermal conversion substance coated on the surface;

[0059] 3) mixing the hydrophilic polymer material chitosan and water at a mass ratio of 1:15 to form a hydrophilic polymer solution, and then adding the cross-linking agent glutaraldehyde and the hydrophilic polymer material at a ratio of 1:7 to the hydrophilic polymer solution to prepare a mixed solution of chitosan and glutaraldehyde;

[0060] 4) applying a mixed solution of chitosan and glutaraldehyde on the outer surface of the high-porosity sponge coated with the photothermal conversion material, and placing it in a constant temperature drying oven at 70° C. for 10 hours after the cross-linking reaction to obtain a cross-linked sample;

[0061] 5) Ultrasonic mixing of carbon dots and dispersant isopropanol at a mass ratio of 1:30 to obtain a high-concentration photothermal conversion material solution;

[0062] 6) A high concentration photothermal conversion material solution is coated on the cross-linked sample surface, and then placed in a constant temperature drying oven and dried at 70°C for 10 hours to obtain an internal and external non-uniform pore structure evaporator with a low porosity interface evaporation layer on the outer layer of the high porosity sponge surface.

[0063] Embodiment 6:

[0064] 1) Ultrasonic mixing of the photothermal conversion material graphene and the dispersant n-butanol at a mass ratio of 1:120 to obtain a low-concentration photothermal conversion material solution;

[0065] 2) coating a low-concentration photothermal conversion substance solution on the surface of a high-porosity polyvinyl alcohol sponge with a porosity of 95% and an internal pore size distribution of 100 to 300 μm, and then placing the sponge in a constant temperature drying oven at 80° C. for 8 hours to obtain a high-porosity sponge with a photothermal conversion substance coated on the surface;

[0066] 3) The hydrophilic polymer material acrylic acid and water are mixed in a mass ratio of 1:20 to form a hydrophilic polymer solution, and then the cross-linking agent glutaraldehyde and the hydrophilic polymer material are added to the hydrophilic polymer solution in a ratio of 1:10 to prepare a mixed solution of acrylic acid and glutaraldehyde; 4) The mixed solution of acrylic acid and glutaraldehyde is applied to the outer surface of the high-porosity sponge coated with the photothermal conversion material, and after the cross-linking reaction, it is placed in a constant temperature drying oven and dried at 80°C for 8 hours to obtain a cross-linked sample;

[0067] 5) Ultrasonic mixing of graphene and dispersant n-butanol at a mass ratio of 1:50 to obtain a high-concentration photothermal conversion material solution;

[0068] 6) A high concentration photothermal conversion material solution is coated on the cross-linked sample surface, and then placed in a constant temperature drying oven and dried at 80°C for 8 hours to obtain an internal and external non-uniform pore structure evaporator with a low porosity interface evaporation layer on the outer layer of the high porosity sponge surface.

[0069] Embodiment 7:

[0070] 1) Ultrasonic mixing of carbon black as a photothermal conversion material and ethanol as a dispersant at a mass ratio of 1:200 to obtain a low-concentration photothermal conversion material solution;

[0071] 2) coating a low-concentration photothermal conversion substance solution on the surface of a high-porosity polyurethane sponge with a porosity of 99% and an internal pore size distribution of 100 to 300 μm, and then placing the sponge in a constant temperature drying oven at 70° C. for 10 hours to obtain a high-porosity sponge with a photothermal conversion substance coated on the surface;

[0072] 3) mixing a hydrophilic polymer material acrylamide and water at a mass ratio of 1:30 to form a hydrophilic polymer solution, and then adding a cross-linking agent glutaraldehyde and the hydrophilic polymer material at a ratio of 1:15 to the hydrophilic polymer solution to prepare a mixed solution of acrylamide and glutaraldehyde;

[0073] 4) applying a mixed solution of acrylamide and glutaraldehyde on the outer surface of the high-porosity sponge coated with the photothermal conversion material, and placing it in a constant temperature drying oven at 70° C. for 10 hours after the cross-linking reaction to obtain a cross-linked sample;

[0074] 5) Ultrasonic mixing of carbon black and dispersant ethanol at a mass ratio of 1:20 to obtain a high-concentration photothermal conversion material solution;

[0075] 6) A high concentration photothermal conversion material solution is coated on the cross-linked sample surface, and then placed in a constant temperature drying oven and dried at 70°C for 10 hours to obtain an internal and external non-uniform pore structure evaporator with a low porosity interface evaporation layer on the outer layer of the high porosity sponge surface.

Claims

1. A method for preparing an evaporator with internal and external non-uniform pore structure, Features The following steps are involved: 1) Ultrasonic mixing the photothermal conversion material and the dispersant at a mass ratio of 1:100 to 1:200 to obtain a low-concentration photothermal conversion material solution; 2) coating a low-concentration photothermal conversion substance solution on the surface of a high-porosity sponge with a porosity of 90-99% and an internal pore size distribution of 100-300 μm, and then placing it in a constant temperature drying oven for drying to obtain a high-porosity sponge with a photothermal conversion substance coated on the surface; 3) mixing a hydrophilic polymer material and water at a mass ratio of 1:15-30 to form a hydrophilic polymer solution, and then adding a cross-linking agent glutaraldehyde and a hydrophilic polymer material to the hydrophilic polymer solution at a ratio of 1:7-15 to prepare a hydrophilic polymer material mixed aqueous solution; 4) Applying a mixed aqueous solution of a hydrophilic polymer material on the outer surface of a high-porosity sponge coated with a photothermal conversion substance, and placing the sponge in a constant temperature drying oven to dry after the cross-linking reaction to obtain a cross-linked sample; 5) Ultrasonic mixing the photothermal conversion material and the dispersant at a mass ratio of 1:20 to 1:50 to obtain a high-concentration photothermal conversion material solution; 6) Applying a high-concentration photothermal conversion material solution on the cross-linked sample surface, and then drying it in a constant temperature drying oven, to obtain an internal and external non-uniform pore structure evaporator having a low-porosity interface evaporation layer outside the high-porosity sponge surface.

2. The method for preparing the evaporator with internal and external non-uniform pore structure according to claim 1, Features: The photothermal conversion material is one or more of carbon black, carbon dots, graphene, and polydopamine.

3. The method for preparing the evaporator with internal and external non-uniform pore structure according to claim 1, Features: The dispersant is one or more of ethanol, isopropanol and n-butanol.

4. The method for preparing the evaporator with internal and external non-uniform pore structure according to claim 1, Features: The high-porosity sponge is melamine sponge, polyvinyl alcohol sponge, melamine sponge or polyurethane sponge.

5. The method for preparing the evaporator with internal and external non-uniform pore structure according to claim 1, Features: The constant temperature drying temperature is 60-80°C, and the constant temperature drying time is 8-12h.

6. The method for preparing the evaporator with internal and external non-uniform pore structure according to claim 1, Features: The hydrophilic polymer material is one or more of polyvinyl alcohol, chitosan, acrylamide, acrylic acid and their derivatives.

7. An evaporator with internal and external non-uniform pore structure manufactured by the preparation method according to any one of claims 1 to 6, Features: The invention comprises a main body with an internal high-porosity structure and an outer low-porosity interface evaporation layer, wherein the porosity of the main body with an internal high-porosity structure is 90-99%, the internal pore size distribution is 100-300 μm, the porosity of the outer low-porosity interface evaporation layer is 70-90%, the pore size distribution is 200 nm-50 μm, and the thickness is 0.1-1 mm.

8. The evaporator with non-uniform internal and external pore structure according to claim 7, Features: The main body of the internal high-porosity structure is a high-porosity melamine sponge, a polyvinyl alcohol sponge, a melamine sponge or a polyurethane sponge.

9. The evaporator with non-uniform internal and external pore structure according to claim 7, Features: The outer low-porosity interface evaporation layer is composed of a gel structure formed by cross-linking of hydrophilic polymer materials and a photothermal conversion substance attached to the gel structure; The hydrophilic polymer material is one or more of chitosan, polyvinyl alcohol, acrylamide, acrylic acid and their derivatives; The photothermal conversion material is one or more of carbon black, carbon dots, graphene, and polydopamine.

Citation Information

Cited By

  • Solar distiller with separated functions and preparation method thereof

    CN121894733A