A polyaniline nanorod-shaped conductive polymer material and preparation method thereof
By using aromatic ring structure dye as a guide agent, the polyaniline morphology is adjusted, and the problems of entanglement and insufficient conductivity of polyaniline materials with high aspect ratio are solved, and good dispersion and high conductivity in various solvents are achieved. The conductivity has been significantly improved.
Patent Information
- Application Number
- CN202410574365.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-10
AI Technical Summary
The high-level diameter synthesized in the prior art is easier to tangle than polyaniline materials, lack processability, and the addition of dispersant damages electrical conductivity, making it difficult to disperse in the solvent, limiting the processing performance of the material.
Use dyes with aromatic ring structure as structural guides to adjust the morphology of polyaniline, improve its dispersion and electrical properties, and use a variety of organic aromatic compounds as one-dimensional hard templates by adjusting the ratio of oxidant, structural guides and monomers. Synthesize high-performance polyaniline microtubules.
The outstanding dispersion and excellent conductivity of polyaniline nanorod-shaped materials in various solvents are achieved, with a conductivity of 10 to 20 times that of ordinary polyaniline materials. The material shows a tendency to self-assemble under specific acidic conditions, forming a nanorod-shaped Structure, the groups on the surface are closely bound to the aniline monomer through hydrogen bonding and π-π stacking, promoting the gradual accumulation of polyaniline on its surface.
Smart Images

Figure CN118240208B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of conductive polymer materials, and in particular relates to a polyaniline nanorod-shaped conductive polymer material and a preparation method thereof. Background Art
[0002] Conductive polymers have attracted much attention due to their outstanding performance in various functions from insulators to conductors, while maintaining the mechanical properties and processing convenience of traditional polymers. Polyaniline is considered to be one of the most promising conductive polymers due to its unique physical and electrochemical properties. Different forms of polyaniline nanostructures have been used in many fields, covering adsorbents, chemical sensors, biosensors, electrocatalysis, supercapacitors, and battery electrode materials. Among polyaniline nanostructures, polyaniline with a high aspect ratio has attracted widespread attention due to its advantage of one-dimensional morphology in device applications.
[0003] At present, there are many methods dedicated to the synthesis of polyaniline with high aspect ratio, of which two methods are the most common. One is the template-free self-assembly method, which allows aniline monomers and oxidants to react spontaneously at the interface between two immiscible liquids, thereby inducing the formation of polyaniline with high aspect ratio. Another method is to use a one-dimensional structure directing agent, by which the morphology and physicochemical properties of polyaniline can be effectively adjusted, thereby controlling the polymerization of aniline. In terms of templates, the existing directing agents are mainly divided into soft templates represented by micelle aggregates and hard templates represented by nanotubular materials. However, the high aspect ratio polyaniline synthesized by the current common methods still has some defects due to its unique structure. For example, most one-dimensional polyanilines prepared using existing synthesis techniques are easy to entangle together, resulting in the lack of processability of the material and difficulty in dispersing in solvents. Dispersants have been used in recent studies to improve the dispersibility of polyaniline. However, the addition of a large amount of dispersant will significantly damage the conductivity of polyaniline, thereby severely limiting the processing performance of the material. Therefore, developing a high aspect ratio polyaniline with both high conductivity and excellent dispersion properties remains a challenging and necessary task. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a polyaniline nanorod-shaped conductive polymer material and a preparation method thereof, and to use a dye with an aromatic ring structure as a structure directing agent to adjust the polyaniline morphology and improve the dispersibility and electrical properties of the polyaniline material.
[0005] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] A polyaniline nanorod-shaped conductive polymer material comprises the following raw materials in parts by weight:
[0007] 50-70 parts of solvent, 0.01-1 parts of structure directing agent, 0.1-0.5 parts of monomer, 0.1-10 parts of oxidant, 0.1-10 parts of dopant.
[0008] In some embodiments, the solvent is selected from at least one of distilled water, ethanol, dimethyl sulfoxide, dimethylformamide, and N-methylpyrrolidone.
[0009] In some other embodiments, the solvent is preferably distilled water.
[0010] In some embodiments, the structure directing agent is selected from at least one of eosin Y, fuchsin, neutral red, oil red O, safranin, and phenol safranin.
[0011] In some other embodiments, the structure directing agent is preferably Eosin Y.
[0012] It should be noted that eosin Y, fuchsin, neutral red, oil red O, safranin or phenol safranin used in the present invention are common organic dyes, which are currently mainly used in histology and cytology in biological staining, but under acidic conditions, their unique structure can form a high-quality colloidal one-dimensional template structure, which can adjust the morphology of polyaniline to enhance its conductivity and dispersibility.
[0013] In some embodiments, the monomer is preferably aniline or aniline hydrochloride.
[0014] In some other embodiments, the monomer is preferably aniline hydrochloride.
[0015] In some embodiments, the oxidant is selected from at least one of ferric chloride, hydrogen peroxide, potassium persulfate, ammonium persulfate, and potassium permanganate.
[0016] In some other embodiments, the oxidizing agent is preferably ammonium persulfate.
[0017] In some embodiments, the dopant is selected from at least one of hydrochloric acid, sulfuric acid, sulfosalicylic acid, p-toluenesulfonic acid, and 1,5-naphthalene disulfonic acid.
[0018] In some other embodiments, the doping agent is preferably hydrochloric acid.
[0019] A method for preparing a polyaniline nanorod-shaped conductive polymer material comprises the following preparation steps:
[0020] S1: dissolving the monomer in a reaction solvent and stirring to form a mixed solution A;
[0021] S2: dissolving the structure directing agent in the mixed solution A and stirring to form a mixed solution B;
[0022] S3: dissolving the dopant in the mixed solution B and stirring to form a mixed solution C;
[0023] S4: dissolving the oxidant in the mixed solution C, stirring the mixture to react and obtaining a suspension;
[0024] S5: filtering the suspension and washing it with acid solution, drying and grinding to obtain polyaniline nanorod-shaped conductive polymer material.
[0025] In some embodiments, the stirring temperature in S1-S4 is 0-50°C; the stirring time in S2 is 60-200 min; the stirring time in S3 is 10-60 min; and the reaction time in S4 is 20-30 h.
[0026] In some embodiments, the acid in S5 is selected from at least one of hydrochloric acid or sulfuric acid.
[0027] In some embodiments, the drying temperature in S5 is 50-120° C., and the drying time is 30-120 min / h.
[0028] The present invention has the following beneficial effects:
[0029] 1. The present invention adjusts the mass fractions of oxidants, structure-directing agents and monomers, and uses a variety of organic aromatic compounds as one-dimensional hard templates to synthesize high-performance polyaniline microtubes. Compared with ordinary polyaniline materials, polyaniline microtubes can be more effectively dispersed in water and other organic solvents.
[0030] 2. The polyaniline nanorod-shaped conductive polymer material provided by the present invention can show outstanding dispersibility and excellent conductive properties in a variety of solvents. Aromatic ring structure dyes show a tendency to self-assemble under specific acidic conditions to form nanorod-shaped structures. The groups on the surface of these nanorods are tightly combined with aniline monomers through interactions such as hydrogen bonds and π-π stacking, which promotes the gradual accumulation of polyaniline on its surface. The unique nanorod-shaped structure is more conducive to electrical conductivity, and its electrical conductivity is 10 to 20 times that of ordinary polyaniline materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The structures of eosin Y, fuchsin, neutral red, oil red O, safranin, and phenol safranin are shown;
[0032] Figure 2 This is a measurement diagram of the nanorod-like structure of the polyaniline nanorod-like conductive polymer material of Example 1;
[0033] Figure 3 This is a diagram of the nanorod-like structure of the polyaniline nanorod-like conductive polymer material of Example 1;
[0034] Figure 4 This is a nanoparticle state diagram of the polyaniline nanorod-shaped conductive polymer material of Comparative Example 1;
[0035] Figure 5This is a dispersion diagram of the polyaniline nanorod-shaped conductive polymer material of Example 1 in different organic solvents. In the figure, 1 to 6 are organic solvents, respectively, including dichloromethane, acetonitrile, dioxane, tetrahydrofuran, ethanol, and methanol. DETAILED DESCRIPTION
[0036] The present invention will be further described in detail below in conjunction with the accompanying drawings. The embodiments described with reference to the accompanying drawings are exemplary and intended to explain the present invention, but should not be construed as limiting the present invention.
[0037] Example 1
[0038] 50 parts of distilled water, 0.5 parts of eosin Y, 2 parts of aniline hydrochloride, 0.1 parts of hydrochloric acid, and 20 parts of ammonium persulfate.
[0039] A method for preparing a polyaniline nanorod-shaped conductive polymer material comprises the following preparation steps:
[0040] S1: Dissolve 2 parts of aniline hydrochloride in 50 parts of distilled water and stir at 25°C to form a transparent light green mixed solution A;
[0041] S2: Dissolve 0.5 parts of eosin Y in mixed solution A and stir at 25°C for 60 min to form a uniform, deep red mixed solution B;
[0042] S3: Dissolve 0.1 parts of hydrochloric acid in mixed solution B and stir at 25°C for 10 minutes to form mixed solution C;
[0043] S4: dissolving 20 parts of ammonium persulfate in the mixed solution C, stirring and reacting at 25°C for 24 hours to obtain a suspension;
[0044] S5: The suspension was filtered and washed with hydrochloric acid, and dried at 80°C for 80 min. , The polyaniline nanorod-shaped conductive polymer material was obtained by grinding.
[0045] Example 2
[0046] The preparation steps are the same as those in Example 1, except that the mass fraction of Eosin Y is 0.25 parts.
[0047] Example 3
[0048] The preparation steps are the same as those in Example 1, except that the mass fraction of eosin Y is 0.125 parts.
[0049] Example 4
[0050] The preparation steps are the same as those in Example 1, except that the mass fraction of eosin Y is 0.0625 parts.
[0051] Example 5
[0052] The preparation steps are the same as those in Example 1, except that eosin Y is replaced by phenol saffron, and the mass fraction of phenol saffron is 0.125.
[0053] Example 6
[0054] The preparation steps are the same as those in Example 1, except that ammonium persulfate is replaced by ferric chloride, and the mass fractions are the same as those in Example 3.
[0055] Example 7
[0056] The preparation steps are the same as those in Example 1, except that eosin Y is replaced by fuchsin, and the mass fraction of fuchsin is 0.125 parts.
[0057] Example 8
[0058] The preparation steps are the same as those in Example 1, except that eosin Y is replaced by neutral red, and the mass fraction of neutral red is 0.125 parts.
[0059] Example 9
[0060] The preparation steps are the same as those in Example 1, except that Eosin Y is replaced by Oil Red O, and the mass fraction of Oil Red O is 0.125 parts.
[0061] Example 10
[0062] The preparation steps are the same as those in Example 1, except that eosin Y is replaced by safranin, and the mass fraction of safranin is 0.125 parts.
[0063] Comparative Example 1
[0064] The preparation steps are the same as those in Example 1, except that no structure directing agent is added.
[0065] The polyaniline nanorod-shaped conductive polymer materials prepared in Examples 1-10 and Comparative Example 1 were tested for their microscopic morphology using a scanning electron microscope (SEM), their conductivity using a four-probe method, and their Zeta potential using dynamic light scattering to determine their dispersibility in water. The results are as follows: Figure 2-5 The performance test results are shown in Table 1 and Table 2.
[0066] Figure 1 The chemical structures of eosin Y, fuchsin, neutral red, oil red O, safranin, and phenol safranin are shown, all of which contain aromatic ring structures; Figure 2 , 3 The polyaniline nanorod-like conductive polymer material obtained in Example 1 is a nanorod-like structure of about 250 nm, indicating that the present invention can produce a polyaniline conductive polymer material with a nanorod-like structure; Figure 4 It shows that the polyaniline powder prepared in Comparative Example 1 is nanoparticles with a diameter of about 50 nm, and does not form a nanorod-like structure; Figure 5It shows that the polyaniline nanorod-shaped conductive polymer material prepared in Example 1 can be dispersed in different organic solvents.
[0067] Table 1 Characterization results of Examples 1-6
[0068]
[0069] Note: Some organic solvents include six widely representative organic solvents such as dichloromethane, acetonitrile, dioxane, tetrahydrofuran, ethanol and methanol.
[0070] Table 2 Characterization results of Examples 7-10 and Comparative Example 1
[0071]
[0072]
[0073] Note: Some organic solvents include six widely representative organic solvents such as dichloromethane, acetonitrile, dioxane, tetrahydrofuran, ethanol and methanol.
[0074] Through the analysis of Table 1, compared with Comparative Example 1, the water dispersibility of the polyaniline nanorod-shaped conductive polymer materials of Examples 1-10 is significantly improved, and the Zeta potential in water is more than 30mV, indicating that these materials can form a stable colloidal solution in water. The research results of Examples 1-10 show that the addition of an appropriate amount of eosin Y or other aromatic ring structure dyes can effectively improve the conductivity of the polyaniline nanorod-shaped conductive polymer material, up to 33S / cm, which is 66 times that of Comparative Example 1. However, too much or too little structure directing agent will lead to a decrease in conductivity. From the data in Table 1, it can be seen that when the structure directing agent is 0.125, the conductivity of the polyaniline nanorod-shaped conductive polymer material is the best.
[0075] The analysis of Examples 1-10 and Comparative Example 1 shows that after adding eosin Y or other aromatic ring structure dyes, Examples 1-10 all form nanorod-like structures. According to Examples 1-4, it can be seen that as the amount of eosin Y added decreases, the length of the nanorods gradually decreases. In other organic solvents (dichloromethane, acetonitrile, dioxane, tetrahydrofuran, ethanol, methanol), the nanorod-like polyaniline of all Examples can be well dispersed, showing excellent dispersibility, while the dispersibility of the polyaniline powder of Comparative Example 1 in other solvents is relatively poor.
[0076] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A polyaniline nanorod-shaped conductive polymer material, characterized in that: Including the following raw materials by mass: 50-70 parts of solvent, 0.01-1 parts of structure directing agent, 0.1-0.5 parts of monomer, 0.1-10 parts of oxidant, 0.1-10 parts of dopant; The structure directing agent is selected from at least one of eosin Y, fuchsin, neutral red, oil red O, safranin, and phenol safranin; the solvent is distilled water; the monomer is aniline or aniline hydrochloride; the oxidant is selected from at least one of ferric chloride and ammonium persulfate; the doping agent is hydrochloric acid; The polyaniline nanorod-shaped conductive polymer material is prepared by the following steps: S1: dissolving the monomer in a reaction solvent and stirring to form a mixed solution A; S2: dissolving the structure directing agent in the mixed solution A and stirring to form a mixed solution B; S3: dissolving the dopant in the mixed solution B and stirring to form a mixed solution C; S4: dissolving the oxidant in the mixed solution C, stirring the mixture to obtain a suspension; S5: filtering the suspension and washing it with an acid solution, drying and grinding it to obtain a polyaniline nanorod-shaped conductive polymer material; Among them, the stirring temperature in S1-S4 is 0-50°C; in S2, the stirring time is 60-200min; in S3, the stirring time is 10-60min; in S4, the reaction time is 20-30h.
2. The polyaniline nanorod-shaped conductive polymer material according to claim 1, characterized in that: In S5, the acid solution is selected from at least one of hydrochloric acid and sulfuric acid.
3. The polyaniline nanorod-shaped conductive polymer material according to claim 1, characterized in that: In S5, the drying temperature is 50-120° C., and the drying time is 30-120 min.