A low temperature connection method for silicon carbide and heat dissipation copper plate

Through the combination of magnetron sputtering technology and SnCu or SnAg eutectic solder, the low-temperature connection between silicon carbide and heat-sinking copper plate is achieved, solving the damage problem of high-temperature connection to power devices, reducing welding temperature and process complexity, and improving connection reliability and productivity.

CN118344170BActive Publication Date: 2024-11-29ANHUI POLYTECHNIC UNIV

Patent Information

Application Number
CN202410273802.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-11
Publication Date
2024-11-29
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

In the prior art, the metallization temperature of silicon carbide and heat dissipation copper plates is high, the process is complex, the welding temperature is high, and the welding cycle is long, which causes damage to the power devices and makes it difficult to achieve reliable low-temperature connections.

Method used

By pretreating and removing impurities on the surface of silicon carbide, using magnetron sputtering technology to sputter Cr and Ag metal films, followed by vacuum brazing using SnCu or SnAg eutectic solder to achieve low temperature connection, and the welding temperature is controlled at 250-280℃ , the insulation time is 5 to 10 minutes.

Benefits of technology

It has achieved the reduction of metallization temperature, simplified process, reduced energy consumption, and prepared high-quality metallized films, with low welding temperature and short cycle, suitable for continuous production, reducing production costs, and increasing SiC ceramics and Cu metals Low temperature connection reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118344170B_ABST
    Figure CN118344170B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of dissimilar material connection, and specifically to a low-temperature connection method for silicon carbide and a heat dissipation copper plate, wherein the method comprises pre-treating and removing impurities from the SiC surface, then metallizing the pre-treated SiC surface by sputtering two layers of metal films of Cr and Ag, and finally assembling the metallized SiC and the copper plate with SnCu or SnAg eutectic solder and then vacuum brazing; wherein, when the SiC surface is metallized, the temperature of the SiC substrate is heated to 100-200°C; the brazing temperature is 250-280°C, and the holding time is 5-10 minutes. The present invention aims to realize the low-temperature reliable connection between SiC ceramics and metal Cu, and on the one hand, provides technical support for the application of SiC power devices in electronic packaging, and on the other hand, provides design ideas for the low-temperature brazing technology of difficult-to-weld and difficult-to-wet materials such as ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of connecting dissimilar materials, and in particular to a low-temperature connection method for silicon carbide and a heat dissipation copper plate. Background Art

[0002] Silicon carbide (SiC) ceramics have excellent properties such as small thermal expansion coefficient, strong oxidation resistance, high thermal conductivity, good wear resistance, and good thermal stability. They are widely used in aerospace, nuclear energy, machinery, microelectronics and other fields. Moreover, because SiC ceramics have high thermal conductivity and the thermal expansion coefficient (CTE) matches well with semiconductor chips such as Si, they are often used as ceramic packaging materials in power devices and have a wide range of application needs in the field of electronic packaging. In the actual application of electronic packaging, in order to meet the requirements of conduction and heat dissipation, SiC ceramics are usually required to be connected to a heat dissipation copper plate or a copper-clad ceramic (DBC) substrate. In order to avoid damage to certain power devices caused by high-temperature connection, it is necessary to achieve a low-temperature reliable connection between SiC and the Cu substrate. Therefore, it is of great significance to develop a reliable low-temperature connection technology for silicon carbide and heat dissipation copper plates.

[0003] At present, the methods used for connecting SiC and Cu in production mainly include active solder method and Mo-Mn method. Active solder method is also called direct soldering method. Generally, active elements or rare earth elements (Ti, Al, Zr, Cr, In, etc.) are introduced into traditional solder for brazing. In order to stimulate the activity of the elements, a higher temperature is usually required. The most commonly used AgCuTi solder has a welding temperature of 880℃-960℃. Mo-Mn method is an important method in ceramic metallization technology and is widely used in ceramic-metal connection in the electronics industry. The principle of this method is to use refractory metal powder Mo as the main component, and add a small amount of low melting point Mn, mix it into slurry and apply it on the surface of the treated ceramic substrate, and then sinter it at high temperature in a humidified atmosphere to form a metallization layer. The disadvantages of the traditional Mo-Mn method are high sintering temperature, high energy consumption, complex process, and lack of activator in the formula resulting in low sealing strength. Even though these two ceramic-metal connection methods are still widely used in industry, for practical applications of electronic packaging, high-temperature connection or high-temperature ceramic metallization methods will cause certain damage to power devices, causing certain functions of electronic devices to fail. Therefore, it is urgent to develop a low-temperature connection technology for SiC and Cu with low metallization operating temperature, simple process, high film quality, and easy mass production. Summary of the invention

[0004] In view of this, the purpose of the present invention is to propose a low-temperature connection method for silicon carbide and a heat dissipation copper plate to solve the problems of high metallization temperature, complex metallization process, high welding temperature and long welding cycle in the prior art.

[0005] Based on the above purpose, the present invention provides a low-temperature connection method for silicon carbide and a heat dissipation copper plate, wherein the method comprises the following steps: firstly pre-treating the SiC surface to remove impurities, then metallizing the pre-treated SiC surface by sputtering two layers of metal films of Cr and Ag, and finally assembling the metallized SiC and the copper plate using SnCu or SnAg eutectic solder and then vacuum brazing them; wherein, when the SiC surface is metallized, the temperature of the SiC substrate is heated to 100-200°C; the brazing temperature is 250-280°C, and the insulation time is 5-10 minutes.

[0006] Preferably, the pretreatment and impurity removal method is to remove the oxide layer and impurities on the surface of the SiC and Cu plates by mechanical grinding, and then remove surface stains by ultrasonic cleaning.

[0007] Furthermore, the working gas used in the SiC surface metallization treatment is 20-50 mL / min of argon gas with a purity of 99.99%, the SiC substrate is heated to 100-200° C., the sputtering vacuum is 0.3-0.6 Pa, the sputtering power is 100-200 W, and the sputtering time is 10-60 min.

[0008] Preferably, the sputtering is performed using a dual-target magnetron sputtering apparatus.

[0009] Preferably, the dual-target head magnetron sputtering apparatus uses a high-purity Cr target with a purity of ≥99.995% and a high-purity Ag target with a purity of ≥99.995%.

[0010] Preferably, the thickness of the sputtered Cr metal film is 200 nm, and the thickness of the Ag metal film is 1000-2000 nm.

[0011] Preferably, the heating rate of the brazing is 5 to 10° C. / min.

[0012] Preferably, the thickness of the brazing welding sheet is 0.10-0.15 mm.

[0013] Preferably, the substrates of the silicon carbide and the heat dissipation copper plate are respectively made of pressureless sintered silicon carbide ceramic and oxygen-free copper plate.

[0014] Beneficial effects of the present invention:

[0015] 1. The present invention uses magnetron sputtering technology to achieve SiC ceramic surface metallization, with low metallization temperature, simple process, low energy consumption, and prepares high-quality metallized films for low-temperature brazing.

[0016] 2. The present invention adopts SnCu or SnAg eutectic solder, and the welding temperature is much lower than the brazing temperature of AgCu active solder, thus realizing low-temperature connection between SiC ceramic and Cu metal. The welding temperature is low, the welding cycle is short, and it is suitable for continuous production, which can effectively reduce production costs.

[0017] 3. On the one hand, the present invention provides technical support for the application of SiC power devices in electronic packaging, and on the other hand, it provides design ideas for low-temperature brazing technology of difficult-to-weld and difficult-to-wet materials such as ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is the SEM morphology of the film surface in Example 1;

[0020] Figure 2 This is the SEM morphology of the film surface in Example 2;

[0021] Figure 3 This is the SEM morphology of the film surface of Comparative Example 1;

[0022] Figure 4 This is a cross-sectional morphology diagram of the film layer of Example 1 of the present invention;

[0023] Figure 5 This is a cross-sectional morphology diagram of the film layer of Example 2 of the present invention;

[0024] Figure 6 This is the cross-sectional morphology of the film layer in Comparative Example 1;

[0025] Figure 7 This is a SEM morphology image of the SiC-Cu joint of Example 1 of the present invention;

[0026] Figure 8 This is a SEM morphology image of the SiC-Cu joint of Example 2 of the present invention;

[0027] Fig. 9 This is a SEM morphology image of the SiC-Cu joint of Example 3 of the present invention;

[0028] Fig.10 This is the SEM morphology of the SiC-Cu joint of Comparative Example 1;

[0029] Fig.11 This is the SEM morphology of the SiC-Cu joint of Comparative Example 2;

[0030] Fig.12 A comparison chart of shear strength between Examples 1-3 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0031] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should have the common meanings understood by persons having ordinary skills in the field to which the present invention belongs.

[0032] Based on the low-temperature packaging application requirements of silicon carbide power devices, the present invention proposes a low-temperature connection process for silicon carbide ceramics and heat dissipation copper plates. In view of the technical difficulties that silicon carbide ceramics are difficult to be wetted by traditional solders, the thermal expansion coefficient does not match that of metals, and the damage to certain power devices caused by high-temperature connection is avoided, the silicon carbide surface is metallized by magnetron sputtering technology, and SnCu or SnAg eutectic solder is used to perform low-temperature vacuum brazing of silicon carbide and oxygen-free copper, successfully achieving the brazing connection of SiC-Cu. The present invention aims to achieve low-temperature reliable connection between SiC ceramics and metal Cu. On the one hand, it provides technical support for the application of SiC power devices in electronic packaging, and on the other hand, it provides design ideas for low-temperature brazing technology of difficult-to-weld and difficult-to-wet materials such as ceramics.

[0033] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0034] Example 1

[0035] Cr and Ag metal films were sputtered on the SiC surface by magnetron sputtering technology. 30 mL / min of high-purity (99.99%) argon was introduced as the working gas, the vacuum degree was 0.3 Pa, the substrate was heated to 200°C, the sputtering power was 150 W, the Cr layer was sputtered for 10 min, and the Ag layer was sputtered for 40 min. A high-quality metallized film layer on the SiC surface was obtained (see Figure 1 ), the thickness of the Cr layer is 200nm (see Figure 4 ), the thickness of the Ag layer is 1000nm (see Figure 4 ). Then, the assembled SiC and Cu were placed in a brazing furnace for vacuum brazing using SnCu brazing filler metal. The welding temperature was 260°C, the heating rate was 5°C / min, the thickness of the soldering sheet was 0.1mm, and the temperature was kept for 8 minutes. There were no obvious cracks or holes at the brazed joint, and an effective connection between SiC and Cu was achieved. The average shear strength of the joint was 18.6MPa (see Figure 7 ).

[0036] Example 2

[0037] Cr and Ag metal films were sputtered on the SiC surface by magnetron sputtering technology. 50 mL / min of high-purity (99.99%) argon was introduced as the working gas, the vacuum degree was 0.5 Pa, the substrate was heated to 200°C, the sputtering power was 200 W, the Cr layer was sputtered for 10 minutes, and the Ag layer was sputtered for 60 minutes. A high-quality metallized film layer on the SiC surface was obtained (see Figure 2 ), the thickness of the Cr layer is 200nm (see Figure 5 ), the thickness of the Ag layer is 2000nm (see Figure 5 ). Then, the assembled SiC and Cu were placed in a brazing furnace for vacuum brazing using SnCu brazing filler metal. The welding temperature was 275°C, the heating rate was 10°C / min, the thickness of the solder sheet was 0.15mm, and the temperature was kept for 10 minutes. The brazed joint had no cracks or holes, and an effective connection between SiC and Cu was achieved. The average shear strength of the joint was 18.8MPa (see Figure 8 ).

[0038] Example 3

[0039] Cr and Ag metal film layers were sputtered on the SiC surface by magnetron sputtering technology. 50mL / min of high-purity (99.99%) argon was introduced as the working gas, the vacuum degree was 0.5Pa, the substrate was heated to 200℃, the sputtering power was 200W, the Cr layer was sputtered for 10min, and the Ag layer was sputtered for 60min. A high-quality metallized film layer was obtained on the SiC surface, with a Cr layer thickness of 200nm and an Ag layer thickness of 2000nm. The assembled SiC and Cu were then placed in a brazing furnace for vacuum brazing using SnAg solder. The welding temperature was 270℃, the heating rate was 8℃ / min, the solder sheet thickness was 0.1mm, and the temperature was kept warm for 10min. The brazed joint had no cracks or holes, achieving an effective connection between SiC and Cu. The average shear strength of the joint was 15MPa (see Fig. 9 ).

[0040] Comparative Example 1

[0041] Cr and Cu metal films were sputtered on the SiC surface by magnetron sputtering technology. 40 mL / min of high-purity (99.99%) argon was introduced as the working gas, the vacuum degree was 0.6 Pa, the substrate was heated to 100 ° C, the sputtering power was 150 W, the Cr layer was sputtered for 10 minutes, and the Cu layer was sputtered for 20 minutes. A high-quality metallized film layer on the SiC surface was obtained (see Figure 3 ), the thickness of the Cr layer is 200nm (see Figure 6 ), the Cu layer thickness is 400nm (see Figure 6). Then, the assembled SiC and Cu were placed in a brazing furnace for vacuum brazing using pure Sn brazing material. The welding temperature was 260°C, the heating rate was 10°C / min, the thickness of the soldering sheet was 0.1mm, and the temperature was kept for 10 minutes. Micro cracks were found at the brazed joint, and the average shear strength of the joint was 5.6MPa (see Fig.10 ).

[0042] Comparative Example 2

[0043] Cr and Cu metal film layers were sputtered on the SiC surface by magnetron sputtering technology, and 45mL / min of high-purity (99.99%) argon was introduced as the working gas. The vacuum degree was 0.5Pa, the substrate was heated to 150°C, the sputtering power was 180W, the Cr layer was sputtered for 10min, and the Cu layer was sputtered for 60min. The thickness of the Cr layer was 200nm, and the thickness of the Cu layer was 2000nm. The assembled SiC and Cu were then placed in a brazing furnace for vacuum brazing using SnAg solder. The welding temperature was 265°C, the heating rate was 10°C / min, the thickness of the solder was 0.1mm, and the heat preservation was 10min. The average shear strength of the brazed joint was 7.6MPa (see Fig.11 ).

[0044] It can be seen from the above examples that magnetron sputtering technology is used to achieve metallization of SiC ceramic surface, the metallization temperature is relatively low, the process is simple, the energy consumption is low, and a high-quality metallized film for low-temperature brazing is prepared. Using SnCu or SnAg eutectic brazing material, the welding temperature is much lower than the brazing temperature of AgCu active brazing material, and low-temperature connection of SiC ceramic and Cu metal is achieved. The welding temperature is low and the welding cycle is short, which is suitable for continuous production and can effectively reduce production costs.

[0045] Those skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the present invention is limited to these examples; under the concept of the present invention, the technical features in the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A low temperature connection method for silicon carbide and a heat dissipation copper plate, characterized in that: The method comprises the following steps: firstly pre-treating the SiC surface to remove impurities, then performing metallization treatment on the pre-treated SiC surface by sputtering two layers of metal films of Cr and Ag, and finally adopting SnCu or SnAg eutectic solder to assemble the metallized SiC and a copper plate and then perform vacuum brazing. When the SiC surface is metallized, the temperature of the SiC substrate is heated to 100-200°C; the brazing temperature is 250-280°C, and the holding time is 5-10 minutes; the thickness of the sputtered Cr metal film is 200nm, and the thickness of the Ag metal film is 1000-2000nm.

2. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 1, characterized in that: The method for pretreatment and impurity removal is to remove the oxide layer and impurities on the surface of the SiC and Cu plates by mechanical grinding, and then remove surface stains by ultrasonic cleaning.

3. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 1, characterized in that: The working gas used in the SiC surface metallization treatment is 20-50 mL / min of argon gas with a purity of 99.99%, the sputtering vacuum is 0.3-0.6 Pa, the sputtering power is 100-200 W, and the sputtering time is 10-60 min.

4. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 3, characterized in that: The sputtering is performed using a dual-target magnetron sputtering apparatus.

5. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 4, characterized in that: The dual-target head magnetron sputtering instrument adopts a high-purity Cr target with a purity of ≥99.995% and a high-purity Ag target with a purity of ≥99.995%.

6. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 1, characterized in that: The heating rate of the brazing is 5-10°C / min.

7. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 1, characterized in that: The thickness of the brazing welding sheet is 0.10-0.15 mm.

8. The low temperature connection method of silicon carbide and heat dissipation copper plate according to claim 1, characterized in that: The substrates of the silicon carbide and the heat dissipation copper plate are respectively made of pressureless sintered silicon carbide ceramic and oxygen-free copper plate.

Citation Information

Patent Citations

  • Lid for functional part and process for producing the same

    CN101529583A

  • LED (light emitting diode) packaged based on zinc oxide-bismuth oxide composite ceramic substrate and preparation method thereof

    CN103050608A

Cited By

  • YSZ ceramic and aluminum-silicon alloy low-temperature connection glass soldering paste and connection method

    CN121107707A