Defect-rich high entropy oxide catalyst and preparation method and application thereof
By using defect-rich high-entropy oxide catalysts in methane catalytic oxidation, using the synergistic action of multiple metal elements and colloid mill dispersion technology, the problem of poor stability of existing catalysts at high temperatures is solved, and the efficiency of methane catalytic oxidation is achieved and long-term stability reduces environmental pollution.
Patent Information
- Application Number
- CN202410561086.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-05-08
AI Technical Summary
The existing methane catalytic oxidation catalysts are prone to sintering at high temperatures, have poor thermal stability, and are expensive in precious metal catalysts, making them difficult to apply on a large scale in the industry. Traditional direct combustion produces high-temperature by-product NOx, which has a great impact on the environment.
Using defect-rich high-entropy oxide catalyst, a metal salt solution of five to seven metal elements, including Mn, Fe, Co, Ni, Cu, Y, Zr and Al, is colloidally dispersed in an alkaline solution to form an amorphous shape. High-entropy oxides combine the synergistic effect of redox and coprecipitation to achieve atomic uniform dispersion of metal elements and abundant active sites, and use colloid mill dispersion technology to achieve rapid preparation and mass production of catalysts.
The high catalytic activity and long-term stability of methane catalytic oxidation reaction are achieved, the generation of secondary pollution is reduced, and new efficient and safe catalytic combustion treatment technology is provided, suitable for methane combustion under industrial conditions.
Smart Images

Figure CN118454665B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a defect-rich high-entropy oxide catalyst and a preparation method and application thereof. Background Art
[0002] Methane is one of the main components of natural gas. Due to its high calorific value and abundant reserves, it is widely used in energy production, natural gas vehicle fuel, chemical synthesis and industrial production. However, methane emissions will cause many environmental problems. On the one hand, as a greenhouse gas, methane has a global warming potential 40 times that of CO2; on the other hand, methane is also an air pollutant, which will have an adverse effect on air quality and human health. Traditional methane direct combustion purification requires a high temperature reaction and is accompanied by the production of high-temperature byproducts such as NO. x In contrast, the cleaner, more efficient, safer and more feasible catalytic combustion treatment technology uses efficient and stable catalysts to completely convert methane into CO2 and H2O, and reduce the generation of secondary pollution.
[0003] The reaction equation for catalytic combustion of methane is as follows:
[0004] CH4(g)+2O2(g)→CO2(g)+2H2O(l)
[0005]
[0006] As a highly exothermic reaction, methane oxidation is thermodynamically feasible, but the tetrahedral structure of the methane molecule and the high-energy symmetrical CH bond (439 kJ / mol) require methane to be activated and participate in the reaction at high temperatures. Therefore, in order to achieve a higher reaction rate and avoid secondary pollution caused by high temperatures, the ideal reaction temperature range should be controlled between 300-800 ° C. In addition, under actual industrial conditions, methane gas usually contains components such as sulfur, chlorine, and water vapor, which are easy to bind to the active sites of the catalyst and cause the catalyst to deactivate. Therefore, it is of great significance to develop a methane combustion catalyst with multiple active sites and high thermal stability.
[0007] The catalysts currently used for catalytic oxidation of methane mainly include supported precious metal catalysts, non-precious metal oxide catalysts, etc. Although precious metal catalysts have high activity at low temperatures, problems such as easy sintering at high temperatures, poor thermal stability, and high prices limit their large-scale industrial application. The various valence states and abundant defect sites of transition metals in metal oxides can provide excellent redox properties and oxygen storage capacity for methane oxidation catalysts. It is reported that transition metal elements and rare earth elements, such as Co, Ni, Mn, Cu, Fe, Ce, Zr, Y and other elements, have good methane catalytic combustion activity. The use of the multi-element synergistic effect in high-entropy oxides can reasonably achieve precise control of catalyst components, and the inherent high structural stability of high-entropy oxides can achieve long-term operation of methane combustion reactions under high temperature conditions. Therefore, it is urgent to develop a high-entropy oxide catalyst for methane oxidation to solve the above problems. Summary of the invention
[0008] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a defect-rich high-entropy oxide catalyst and a preparation method and application thereof. The prepared high-entropy oxide can achieve atomic-level uniform dispersion of five to seven metal elements, and its element types and composition are adjustable, thereby achieving high catalytic activity and long-term stability in the catalytic oxidation reaction of methane.
[0009] The technical solution of the present invention is:
[0010] In a first aspect, the present invention provides a method for preparing a defect-rich high entropy oxide catalyst, comprising the following steps:
[0011] S1. After mixing the metal salt solution and the alkaline solution, the mixture is dispersed by a colloid mill to obtain a precipitate; wherein the metal salt solution is a solution obtained by uniformly mixing metal salts corresponding to 5-7 elements of Mn, Fe, Co, Ni, Cu, Y, Zr and Al in deionized water, and the elements are mixed in equal molar ratios;
[0012] S2: washing the precipitate of step S1 with deionized water until the pH is neutral, and then drying to obtain a precursor material;
[0013] S3 grinds the precursor material of step S2 into powder, and then calcines it to obtain an amorphous defect-rich high entropy oxide catalyst.
[0014] Preferably, in step S1, the metal salt corresponding to the Mn element in the metal salt solution is potassium permanganate, nitrate or acetate, and the metal salts corresponding to other elements are nitrate or acetate.
[0015] Preferably, in step S1, the alkaline solution is sodium hydroxide solution, sodium carbonate solution or ammonia solution.
[0016] Preferably, in step S1, the molar ratio of the alkaline compound to all metal salts in the alkaline solution is 1.5-4:1.
[0017] Preferably, in step S1, the dispersing time of the colloid mill disperser is 1-5 min.
[0018] Preferably, in step S2, the drying temperature is 60-100°C and the drying time is 6-12h.
[0019] Preferably, in step S3, the calcination conditions are to heat the material from room temperature to 400-600°C at a heating rate of 5-10°C / min in an air atmosphere for 3-6 hours. Too high a calcination temperature will affect the amorphous structure of the high entropy oxide, thereby affecting the surface defect sites and reducing the catalytic performance of methane combustion.
[0020] In a second aspect, the present invention provides a defect-rich high entropy oxide catalyst prepared by the above preparation method.
[0021] In a third aspect, the present invention also provides the use of the above-mentioned defect-rich high entropy oxide catalyst in the catalytic oxidation of methane.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention can reduce the size of the prepared catalyst particles and increase the specific surface area through the synergistic effect of redox and coprecipitation during the catalyst synthesis process, and further combine the colloidal mill dispersion technology, so as to achieve the formation of multi-element high dispersion and rich defects of high entropy metal oxides. The high entropy oxide prepared by the present invention can achieve atomic-level uniform dispersion of five to seven metal elements, and its element types and composition are both adjustable, which can provide abundant active sites for the catalytic oxidation reaction of methane, and realize the controllable preparation of new defect-rich high entropy oxide catalysts. In addition, the synergistic effect between multiple specific elements can regulate the electronic structure and physicochemical properties of the catalyst, and can effectively promote the activation and deep oxidation of CH bonds that are difficult to degrade in methane, thereby achieving high catalytic activity and long-term stability in the catalytic oxidation reaction of methane.
[0024] 2. The colloid mill dispersion technology adopted in the present invention can realize the rapid preparation and batch production of the catalyst, and provides a new preparation method and design idea for realizing a high-entropy oxide catalyst with small grain size, low cost, convenient and efficient preparation for the catalytic oxidation of methane. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the XRD spectra of the catalysts of Examples 1-5 and Comparative Examples 1-3.
[0026] Figure 2It is the activity diagram of the methane complete oxidation reaction of the catalysts of Example 5 and Comparative Examples 1-3.
[0027] Figure 3 These are the evaluation results of the catalysts of Example 5 and Comparative Examples 2-3 on the stability of catalytic complete oxidation of methane at 500°C. DETAILED DESCRIPTION
[0028] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0029] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0030] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0031] Example 1
[0032] The preparation method of the defect-rich high entropy oxide catalyst of this embodiment comprises the following steps:
[0033] S1 Take 1mmol potassium permanganate and 21mmol sodium carbonate, dissolve them in 150mL deionized water, record it as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol zirconium acetate and 2mmol aluminum acetate, dissolve them in 750mL deionized water, record it as solution B; mix and stir solutions A and B in a colloid mill for 1min to obtain a precipitate;
[0034] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0035] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 600 °C at a heating rate of 5 °C / min, and maintained for 3 h. After naturally cooling to room temperature, an amorphous defect-rich high entropy oxide catalyst (MnCuFeNiCoZrAl)O was obtained. x .
[0036] Example 2
[0037] The preparation method of the defect-rich high entropy oxide catalyst of this embodiment comprises the following steps:
[0038] S1 Take 1mmol potassium permanganate and 56mmol sodium carbonate, dissolve them in 150mL deionized water, record it as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol zirconium acetate and 2mmol yttrium acetate, dissolve them in 750mL deionized water, record it as solution B; mix and stir solutions A and B with a colloid mill for 3 minutes to obtain a precipitate;
[0039] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0040] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 500 °C at a heating rate of 5 °C / min, and maintained for 4 h. After naturally cooling to room temperature, an amorphous defect-rich high entropy oxide catalyst (MnCuFeNiCoZrY)O was obtained. x .
[0041] Example 3
[0042] The preparation method of the defect-rich high entropy oxide catalyst of this embodiment comprises the following steps:
[0043] S1 Take 1mmol potassium permanganate and 21mmol ammonia solution, dissolve in 150mL deionized water, record as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol yttrium acetate and 2mmol aluminum acetate, dissolve in 750mL deionized water, record as solution B; mix and stir solutions A and B with a colloid mill for 2 minutes to obtain a precipitate;
[0044] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 100° C. for 6 h to obtain a precursor material;
[0045] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 550°C at a heating rate of 10°C / min, and maintained for 6 hours. After naturally cooling to room temperature, an amorphous defect-rich high entropy oxide catalyst (MnCuFeNiCoYAl)O was obtained. x .
[0046] Example 4
[0047] The preparation method of the defect-rich high entropy oxide catalyst of this embodiment comprises the following steps:
[0048] S1 Take 1mmol potassium permanganate and 21mmol sodium hydroxide, dissolve them in 150mL deionized water, record it as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate and 2mmol zirconium acetate, dissolve them in 750mL deionized water, record it as solution B; mix and stir solutions A and B with a colloid mill disperser for 5 minutes to obtain a precipitate;
[0049] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 60° C. for 10 h to obtain a precursor material;
[0050] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 400 °C at a heating rate of 8 °C / min, and maintained for 2 h. After naturally cooling to room temperature, an amorphous defect-rich high entropy oxide catalyst (MnCuFeNiCoZr)O was obtained. x .
[0051] Example 5
[0052] The preparation method of the defect-rich high entropy oxide catalyst of this embodiment comprises the following steps:
[0053] S1 Take 1mmol potassium permanganate and 21mmol sodium hydroxide, dissolve in 150mL deionized water, record as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol yttrium acetate and 2mmol aluminum acetate, dissolve in 750mL deionized water, record as solution B; mix and stir solutions A and B with a colloid mill for 1min to obtain a precipitate;
[0054] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0055] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 600 °C at a heating rate of 5 °C / min, and maintained for 3 h. After naturally cooling to room temperature, an amorphous defect-rich high entropy oxide catalyst (MnCuFeNiCoYAl)O was obtained. x .
[0056] Comparative Example 1
[0057] The preparation method of the conventional methane combustion MnO2 catalyst of Comparative Example 1 comprises the following steps:
[0058] S1: Take 3mmol potassium permanganate and 21mmol sodium hydroxide, dissolve them in 150mL deionized water, record it as solution A; take 5mmol manganese acetate, dissolve it in 750mL deionized water, record it as solution B; mix and stir solutions A and B in a colloid mill for 1min to obtain a precipitate;
[0059] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0060] S3 grinds the precursor material into powder using a mortar, then places it in a muffle furnace under an air atmosphere, heats it from room temperature to 550°C at a heating rate of 5°C / min, maintains it for 3 hours, and naturally cools it to room temperature to obtain a traditional methane combustion MnO2 catalyst.
[0061] Comparative Example 2
[0062] The preparation method of the multi-element non-high entropy oxide catalyst having five crystal phases physically mixed in Comparative Example 2 comprises the following steps:
[0063] S1 Take 21mmol of sodium hydroxide and dissolve it in 150mL of deionized water, which is called solution A; Take 2mmol of copper acetate, 2mmol of iron acetate, 2mmol of nickel acetate and 2mmol of cobalt acetate respectively and dissolve them in 750mL of deionized water, which is called solution BE; Mix solution A and solution BE respectively with a colloid mill and stir for 1min to obtain a precipitate;
[0064] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0065] S3 grinds the precursor material into powder with a mortar, and then places it in a muffle furnace under air atmosphere, and heats it from room temperature to 550°C at a heating rate of 5°C / min, and maintains it for 3h. After naturally cooling to room temperature, traditional methane combustion CuO, Fe2O3, NiO, and Co3O4 catalysts are obtained;
[0066] S4 Physically mix the above-mentioned CuO, Fe2O3, NiO, Co3O4 catalysts and the MnO2 catalyst prepared in Comparative Example 1 according to equal molar ratios of metal elements to obtain a multi-element non-high entropy oxide catalyst having a physical mixture of five crystal phases.
[0067] Comparative Example 3
[0068] The preparation method of the multi-element non-high entropy oxide catalyst having seven crystal phases physically mixed in Comparative Example 3 comprises the following steps:
[0069] S1 Take 21mmol of sodium hydroxide and dissolve it in 150mL of deionized water, which is called solution A; take 2mmol of zirconium acetate and 2mmol of yttrium acetate and dissolve them in 750mL of deionized water, which are called solutions F and G; respectively, mix solution A and solution FG with a colloid mill and stir for 3min to obtain a precipitate;
[0070] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0071] S3: Grind the precursor material into powder using a mortar, then place it in a muffle furnace under air atmosphere, heat it from room temperature to 550°C at a heating rate of 5°C / min, maintain it for 3h, and naturally cool it to room temperature to obtain oxides ZrO2 and Y2O3;
[0072] S4 Physically mix the above-mentioned oxides ZrO2, Y2O3, MnO2 catalyst prepared in Comparative Example 1 and CuO, Fe2O3, NiO and Co3O4 catalysts prepared in Comparative Example 2 in equal molar ratios of metal elements to obtain a multi-element non-high entropy oxide catalyst having a physical mixture of seven crystal phases.
[0073] Figure 1 It is the XRD spectra of the catalysts of Examples 1-5 and Comparative Examples 1-3, which illustrate that the high entropy oxides prepared in Examples 1-5 are all amorphous structures with poor crystallinity and therefore have rich defect structures, while the catalysts prepared in Comparative Examples 1-3 exhibit multiple crystalline phase structures with high crystallinity.
[0074] Comparative Example 4
[0075] The preparation method of the amorphous high entropy oxide catalyst of Comparative Example 4 comprises the following steps:
[0076] S1 Take 1mmol potassium permanganate and 21mmol sodium hydroxide, dissolve them in 150mL deionized water, record it as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol cerium acetate and 2mmol samarium acetate, dissolve them in 750mL deionized water, record it as solution B; mix and stir solutions A and B in a colloid mill for 1min to obtain a precipitate;
[0077] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0078] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 600 °C at a heating rate of 5 °C / min, and maintained for 3 h. After naturally cooling to room temperature, an amorphous high entropy oxide (MnCuFeNiCoCeSm)O was obtained. x .
[0079] Comparative Example 5
[0080] The preparation method of the amorphous high entropy oxide catalyst of Comparative Example 5 comprises the following steps:
[0081] S1 Take 1mmol potassium permanganate and 21mmol sodium hydroxide, dissolve in 150mL deionized water, record as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol bismuth acetate and 2mmol lanthanum acetate, dissolve in 750mL deionized water, record as solution B; mix and stir solutions A and B in a colloid mill disperser for 1min to obtain a precipitate;
[0082] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0083] S3 grinds the precursor material into powder using a mortar, and then places it in a muffle furnace under air atmosphere, and heats it from room temperature to 600 °C at a heating rate of 5 °C / min, and maintains it for 3 h. After cooling naturally to room temperature, an amorphous high entropy oxide (MnCuFeNiCoBiLa)O is obtained. x .
[0084] Comparative Example 6
[0085] The difference from Example 1 is that in step S1, solutions A and B are mixed and stirred with a magnetic rotor for 1 min at a rotation speed of 500 r / min to obtain a precipitate.
[0086] Comparative Example 7
[0087] The preparation method of the high entropy oxide catalyst of Comparative Example 7 comprises the following steps:
[0088] S1 Take 1mmol potassium permanganate and 21mmol sodium hydroxide, dissolve in 150mL deionized water, record as solution A; take 3mmol manganese acetate, 4mmol copper acetate, 2mmol iron acetate, 1mmol nickel acetate, 1mmol cobalt acetate, 2mmol zirconium acetate, 2mmol yttrium acetate and 2mmol aluminum acetate, dissolve in 750mL deionized water, record as solution B; mix and stir solutions A and B with a colloid mill disperser for 1min to obtain a precipitate;
[0089] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0090] S3 The precursor material was ground into powder using a mortar and placed in a muffle furnace under air atmosphere, and the temperature was raised from room temperature to 600 °C at a heating rate of 5 °C / min, maintained for 3 h, and naturally cooled to room temperature to obtain an amorphous defect-rich high entropy oxide catalyst (Mn2Cu2FeNi 0.5 Co 0.5 ZrAl)O x .
[0091] Comparative Example 8
[0092] The preparation method of the high entropy oxide catalyst of Comparative Example 8 comprises the following steps:
[0093] S1 Take 1mmol potassium permanganate and 100mmol sodium carbonate, dissolve them in 150mL deionized water, record it as solution A; take 1mmol manganese acetate, 2mmol copper acetate, 2mmol iron acetate, 2mmol nickel acetate, 2mmol cobalt acetate, 2mmol zirconium acetate and 2mmol aluminum acetate, dissolve them in 750mL deionized water, record it as solution B; mix and stir solutions A and B with a colloid mill disperser for 1min to obtain a precipitate;
[0094] S2: washing the precipitate with deionized water three times until the pH of the precipitate supernatant is neutral, and then drying it in an oven at 80°C for 12h to obtain a precursor material;
[0095] S3 The precursor material was ground into powder using a mortar, and then placed in a muffle furnace under air atmosphere, and heated from room temperature to 600 °C at a heating rate of 5 °C / min, and maintained for 3 h. After naturally cooling to room temperature, an amorphous defect-rich high entropy oxide catalyst (MnCuFeNiCoZrAl)O was obtained. x - Excess base.
[0096] Comparative Example 9
[0097] The difference from Example 1 is that in step S3, the calcination temperature is 800°C.
[0098] Catalyst performance evaluation
[0099] A small fixed-bed continuous flow reaction evaluation device was used to evaluate the performance of methane catalytic oxidation. The reactants and products were analyzed using a 7890B gas chromatograph (Agilent), which was equipped with a hydrogen flame ionization detector (FID) for detecting CH4 and a thermal conductivity detector (TCD) for detecting CO2. During the test, 100 mg of a 40-60 mesh catalyst obtained by sieving the pressed tablets was loaded into a quartz tube, and the quartz surfaces were placed in front and behind the catalyst. The reaction temperature was controlled by a programmed temperature reactor, and the thermocouple was located in the center of the catalyst. A mass flow meter was used to control the reaction gas flow. The reaction gas consisted of 1% CH4, 32% O2, and N2 as a balance gas, and was introduced into the catalyst reaction bed at a total flow rate of 50 mL / min, and the space velocity (GHSV) was 30000 mL·g -1 ·h -1 The reaction temperature was 200-650℃, and each temperature point was stabilized for at least 30 minutes before sampling and analysis. The stability measurement was performed at 1% CH4+32% O2 / N2, total flow rate 50mL / min, GHSV=30000mL·g -1 ·h -1 , the reaction temperature is 500°C.
[0100] The methane combustion activity evaluation of the catalysts of Examples 1-5 and Comparative Examples 1-9 at 500°C and the decrease in methane conversion after a 5h stability test are shown in Table 1, and the products are CO2 and H2O.
[0101] Table 1
[0102]
[0103]
[0104] As shown in Table 1, compared with Examples 1-5, the methane conversion rate of the catalysts of Comparative Examples 1-3 decreased, which is attributed to the unique structural property advantages of the high entropy oxide containing multiple elements in the present invention. Compared with Examples 1-5, the methane conversion rate of the catalysts of Comparative Examples 4-5 decreased, which is attributed to the synergistic effect of the specific elements Y, Zr, and Al. Compared with Example 1, the methane conversion rate of the catalysts of Comparative Examples 6-9 decreased, which shows that the colloidal mill dispersion technology, the molar ratio of each metal element, the amount of alkaline compound added, and the calcination temperature in the preparation process can have a significant impact on the performance of the catalyst.
[0105] Figure 2 It is the methane complete oxidation reaction activity diagram of the catalysts of Example 5 and Comparative Examples 1-3, which reflects that the unique structure and properties of the high entropy oxide containing multiple elements of the present invention greatly improve the catalytic performance of the catalyst.
[0106] Figure 3These are the evaluation results of the stability of the catalysts of Example 5 and Comparative Examples 2-3 in catalyzing complete oxidation of methane at 500°C, indicating that the defect-rich high-entropy oxide catalyst prepared by the present invention has excellent thermal stability in the methane combustion reaction.
Claims
1. A method for preparing a defect-rich high entropy oxide catalyst for use in catalytic oxidation of methane, characterized in that: The following steps are involved: S1: mixing a potassium permanganate solution, a metal salt solution and an alkaline solution, and dispersing them using a colloid mill to obtain a precipitate; wherein the metal salt solution is a solution obtained by uniformly mixing metal salts corresponding to Mn, Cu, Fe, Ni, Co, Zr and Al, or Mn, Cu, Fe, Ni, Co, Zr and Y, or Mn, Cu, Fe, Ni, Co, Y and Al, or Mn, Cu, Fe, Ni, Co and Zr, or Mn, Cu, Fe, Ni, Co, Y and Al in deionized water, and the elements are mixed in equal molar ratios; the molar ratio of the alkaline compound to all metal salts in the alkaline solution is 1.5-4:1; S2: washing the precipitate of step S1 with deionized water until the pH is neutral, and then drying to obtain a precursor material; S3 grinds the precursor material of step S2 into powder, and then calcines it to obtain an amorphous defect-rich high entropy oxide catalyst. The calcination conditions are: in an air atmosphere, heating at a heating rate of 5-10°C / min from room temperature to 400-600°C, and the calcination time is 3-6h.
2. The method for preparing a defect-rich high entropy oxide catalyst for use in catalytic oxidation of methane according to claim 1, characterized in that: In step S1, the metal salt corresponding to the Mn element in the metal salt solution is potassium permanganate, nitrate or acetate, and the metal salts corresponding to other elements are nitrate or acetate.
3. The method for preparing a defect-rich high entropy oxide catalyst for use in catalytic oxidation of methane according to claim 1, characterized in that: In step S1, the alkaline solution is a sodium hydroxide solution, a sodium carbonate solution or an ammonia solution.
4. The method for preparing a defect-rich high entropy oxide catalyst for use in catalytic oxidation of methane according to claim 1, characterized in that: In step S1, the dispersing time of the colloid mill disperser is 1-5 minutes.
5. The method for preparing a defect-rich high entropy oxide catalyst for use in catalytic oxidation of methane according to claim 1, characterized in that: In step S2, the drying temperature is 60-100°C and the drying time is 6-12 hours.
6. A defect-rich high entropy oxide catalyst used in catalytic oxidation of methane prepared by the preparation method according to any one of claims 1 to 5.
Citation Information
Patent Citations
Method for preparing copper-based butyraldehyde hydrogenation butanol catalyzer through coprecipitation and spray-drying
CN105107512A
Preparation method and application of porous layered high-entropy oxide with hindered Lewis pair
CN115555030A
Preparation method of high-entropy oxide material for catalytic oxidation of propane gas
CN117299147A