Method for treating scrapped substrate of cadmium telluride photovoltaic module
Through crushing, acid leaching and water washing, the scrap substrates of cadmium telluride photovoltaic modules are processed into conventional glass fragments, which solves the problems of high cost and contamination risk, and achieves efficient processing of small batches and cost savings.
Patent Information
- Application Number
- CN202410367678.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Cadmium telluride photovoltaic module production institutions face high costs and the risk of heavy metal contamination diffusion when processing scrapped substrates. Existing technology is difficult to apply to small batch processing and effectively control pollution.
Using crushing treatment, acid leaching treatment, water washing treatment and detection steps, the scrapped substrates are processed into conventional glass fragments. Through the repeated use of acid leaching liquid and the use of spiral separators, cadmium and tellurium are separated and recovered, reducing processing costs and pollution risks. .
It effectively reduces the warehousing and pollution prevention and control costs of cadmium telluride photovoltaic module production institutions, achieves efficient processing of small batches of scrapped substrates, reduces the risk of heavy metal contamination, and saves material and time costs.
Smart Images

Figure CN118681902A
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic module waste treatment, and in particular to a method for treating a scrapped substrate of a cadmium telluride photovoltaic module. Background Art
[0002] Cadmium telluride photovoltaic modules are thin-film battery modules that convert light energy into electrical energy and are widely used in modern industry and construction. In the production process of cadmium telluride photovoltaic modules, some scrapped glass substrates are inevitably produced. The storage of scrapped substrates requires a lot of space, and there is cadmium telluride film on the scrapped glass substrates. If not handled carefully, it is easy to cause heavy metal pollution and affect the environment.
[0003] In the prior art, the purpose of processing scrapped substrates of cadmium telluride photovoltaic modules is to recover tellurium and cadmium from the substrates, thereby reusing the tellurium and cadmium, or selling them to obtain economic benefits.
[0004] However, for the above-mentioned prior art, due to the limited stock of tellurium and cadmium on the scrapped substrates, it is difficult to obtain sufficient tellurium and cadmium in the process of small-batch processing, and it is often difficult to cover the processing costs. Therefore, the processing in the above-mentioned prior art is only applicable to specialized hazardous goods processing institutions, but not to the production institutions of cadmium telluride photovoltaic modules. For the production institutions of cadmium telluride photovoltaic modules, the storage and transportation of scrapped substrates to hazardous goods processing institutions require expensive storage and transportation costs, and there is a risk of heavy metal pollution spreading. Summary of the invention
[0005] In view of this, the present invention provides a method for processing scrapped substrates of cadmium telluride photovoltaic modules to solve the problem that the production institutions of cadmium telluride photovoltaic modules have high processing costs for scrapped substrates and there is a risk of heavy metal pollution diffusion.
[0006] The present invention provides a method for processing scrapped substrates of cadmium telluride photovoltaic modules, comprising the following steps: crushing treatment, crushing the scrapped substrate to obtain substrate fragments; acid leaching treatment, mixing the substrate fragments with an acid leaching liquid, stirring the reaction for a set time, separating the substrate fragments from the acid leaching liquid to obtain pickled fragments, repeatedly using the acid leaching liquid until it reaches a recycling standard, and then collecting the acid leaching liquid; water washing treatment, washing the pickled fragments with water to obtain quasi-clean fragments, and collecting and storing the washing water; fragment drying, drying the quasi-clean fragments; fragment detection, performing heavy metal index detection on the dried quasi-clean fragments, completing the processing if the processing standard is met, and mixing the quasi-clean fragments with the substrate fragments to wait for re-acid leaching if the processing standard is not met.
[0007] Beneficial effects: The scrapped substrates generated on the production line are easier to handle and more efficiently after being crushed. The substrate fragments are treated with acid leaching to separate the thin film containing cadmium and tellurium attached to the substrate fragments from the substrate, and then washed with water to obtain quasi-clean fragments. The quasi-clean fragments are tested. If they meet the treatment standards, the cadmium residue and tellurium residue on the quasi-clean fragments are no longer hazardous waste standards, but are conventional waste products. They can be collected, stored and taken out according to the standards of ordinary glass fragments. The storage and processing costs are low, which effectively saves corporate costs. Since the main purpose of this method is to process scrapped substrates into quasi-clean fragments of conventional waste standards, rather than recycling cadmium or tellurium, it is suitable for the processing of small batches of scrapped substrates, and can process scrapped substrates in a timely manner, thereby effectively controlling the storage and pollution prevention costs of the production organization of cadmium telluride photovoltaic modules for storing scrapped substrates. In addition, the repeated use of the acid leaching solution can save material costs on the one hand, and on the other hand, it can enrich the cadmium or tellurium on the substrate fragments in the collected acid leaching solution, and then collect and store the collected acid leaching solution and cleaning water in a special container. Compared with the direct storage and pollution control of scrapped substrates, it is more convenient, with lower time and economic costs.
[0008] In an optional embodiment, during the crushing process, the scrapped substrate is crushed into particles with a size less than 2 CM.
[0009] Beneficial effect: Substrate fragments are obtained by crushing the scrapped substrates, and the particle size of the substrate fragments is controlled to be less than 2CM, which is convenient for storage and transportation, and also improves the efficiency of subsequent acid leaching, water washing and drying treatment steps.
[0010] In an optional embodiment, when performing the acid leaching treatment, the substrate fragments are placed in a drum reactor, and the substrate fragments are stirred when the drum of the drum reactor rotates in a first direction, and the broken substrate is discharged from the discharge port of the drum reactor when the drum of the drum reactor rotates in a second direction, and then the pickling fragments are separated from the acid leaching liquid by a spiral separator.
[0011] Beneficial effects: using a drum reactor instead of a reactor to carry out acid leaching treatment on substrate fragments can avoid the situation where substrate fragments accumulate in the reactor and block the lower end discharge port of the reactor, and the drum reactor can be used to directly pour materials through the feed hopper to add materials, and the drum reactor rotates in two directions to stir the substrate fragments and discharge the substrate fragments that have completed the acid leaching treatment from the drum, which is easy to operate, fast in and out, and high in efficiency. In addition, a spiral separator is used to separate the substrate fragments from the acid leaching liquid, and the acid leaching liquid in the spiral separator can continue to separate the thin film on the surface of the substrate fragments. At the same time, the spiral separator gradually lifts the substrate fragments above the liquid level. As the substrate fragments are lifted, most of the acid leaching liquid attached to the surface of the substrate fragments flows back to the bottom of the spiral separator, which is convenient and quick, and reduces the difficulty of cleaning the pickled fragments. The spiral separator is not prone to blockage and jamming, and the separation efficiency of the substrate fragments is stable and reliable, which can make the substrate fragments output evenly.
[0012] In an optional embodiment, when the acid leaching treatment is performed, the acid leaching liquid is sulfuric acid and hydrogen peroxide, wherein the concentration of sulfuric acid is 0.5 mol / L-8 mol / L, and the concentration of hydrogen peroxide is 5%-15%; or, the acid leaching liquid is nitric acid, and the concentration of nitric acid is 30%-65%. During the acid leaching treatment, when the acid leaching liquid is sulfuric acid and hydrogen peroxide, the acid leaching liquid is heated to 40°C-85°C.
[0013] Beneficial effect: The cadmium telluride film attached to the substrate fragments is corroded and oxidized by the acid immersion liquid, so that the cadmium telluride film is separated from the substrate fragments.
[0014] In an optional embodiment, when performing the acid leaching treatment, the liquid-to-solid ratio of the acid leaching liquid to the substrate fragments ranges from 3L:1kg to 10L:1kg, and the reaction time is 0.2 hours to 1 hour.
[0015] Beneficial effects: The liquid-to-solid ratio and reaction time are flexibly adjusted according to the amount of cadmium telluride film attached to the scrapped substrate during actual processing and the number of broken substrates to be processed, which further improves the processing efficiency and saves reagent costs.
[0016] In an optional embodiment, the collected acid extract is diluted 5 to 10 times and then mixed with the cleaning water and stored together.
[0017] Beneficial effects: The collected acid leaching liquid is mixed with the cleaning water and stored together, which reduces the corrosiveness of the collected acid leaching liquid and facilitates storage. The pickling liquid is mixed with the cleaning water after absorption to avoid too much slag during the neutralization process of the concentrated recovered acid solution, and the acid concentration in the reactor is too high, and the amount of the dosing reagent is not easy to control, which affects the reaction effect.
[0018] In an optional embodiment, the acid leaching solution is repeatedly used until the recovery standard is reached when the suspended matter in the acid leaching solution is greater than or equal to 30%.
[0019] Beneficial effect: During the repeated use of the acid leaching solution, the cadmium telluride film is continuously enriched in the acid leaching solution. At this time, the concentration of the effective oxidant component in the acid leaching solution is reduced and the processing capacity is weakened. The acid leaching solution can be recycled to collect the enriched cadmium and tellurium together. On the other hand, it is convenient to ensure the overall concentration of the effective oxidant component of the acid leaching solution in the reaction container when adding new acid leaching solution, thereby ensuring the processing efficiency and quality of the substrate fragments.
[0020] In an optional embodiment, the water washing treatment includes at least a primary water washing and a secondary water washing performed in sequence, and a spiral separator is used to clean the pickled fragments during the primary water washing and the secondary water washing process, and clean water is input 150mm-300mm above the liquid level in the spiral separator so that the clean water flows from the end of the spiral separator to the front end, and compressed air is delivered to the bottom of the spiral separator feed trough used in the primary water washing process.
[0021] Beneficial effect: by setting the primary water washing and the secondary water washing, the pickling fragments are washed twice, so that the pickling liquid attached to the surface of the pickling fragments is cleaned, the pickling fragments are evenly lifted by the spiral separator, and compressed air is delivered at the bottom of the feed tank of the spiral separator to stir the pickling fragments, so that the pickling fragments and the pickling liquid attached to the surface are quickly separated, and then clean water is input from the position near the end of the spiral separator to wash the pickling fragments, and the water flow carries the pickling liquid washed from the pickling fragments back to the feed tank, so that the pickling fragments are gradually cleaned along the ascending path, and then the pickling fragments are further washed by the spiral separator of the secondary water washing, so that most of the pickling liquid and the pickling fragments can be ensured to be separated, and then conventional glass debris waste that does not meet the hazardous waste standards is obtained, which is convenient for stacking and storage by a simple method, or directly sold to ordinary waste recycling units.
[0022] In an optional embodiment, when conducting the fragment detection, take a quasi-clean fragment sample of no less than 2 kg, and oscillate and soak the quasi-clean fragment sample in nitric acid with a pH less than 2 for 18 hours to 22 hours, and the liquid-to-solid ratio of nitric acid to the quasi-clean fragment sample is 10L:1kg. After the treatment, the total cadmium is tested. When the total cadmium is less than 1 mg / L, the quasi-clean fragment meets the treatment standard, otherwise it does not meet the treatment standard.
[0023] Beneficial effect: The standard for hazardous waste is mainly the content of heavy metals in the waste. For scrapped substrates, it is mainly the content of cadmium. Therefore, the total cadmium index in the quasi-cleaning fragments is tested. If it meets the standard, the quasi-cleaning fragments are not hazardous waste and can be taken away directly. If it does not meet the standard, the quasi-cleaning fragments have not been cleaned up and need to be reprocessed and tested again.
[0024] In an optional embodiment, after the collection of the acid leaching liquid is completed, the following steps are also included: tellurium separation, including pretreatment, putting the collected acid leaching liquid or the cleaning water into a container, adjusting the pH value to 2-3, and then adjusting the voltage in the container to 350MV-650MV, reacting for 0.5 hours to 1.5 hours to obtain a tellurium recovery liquid; primary separation, adjusting the pH value of the tellurium recovery liquid to 2.5-3.5, filtering the precipitate to obtain primary crude tellurium and primary filtrate; secondary separation, adjusting the pH value of the primary filtrate to 3.5-4.5, filtering the precipitate to obtain secondary crude tellurium and secondary filtrate; tertiary separation, adjusting the pH value of the secondary filtrate to 4.5-6.5, filtering the precipitate to obtain tertiary crude tellurium and tertiary filtrate; crude tellurium collection, collecting the primary crude tellurium, the secondary crude tellurium and the tertiary crude tellurium respectively.
[0025] Beneficial effects: By graded separation of crude tellurium at different pH values, tellurium can be separated from the solution more thoroughly, and the tellurium content of the primary crude tellurium can reach 40%-85%, the content of the secondary crude tellurium can reach 20%-50%, and the content of the tertiary crude tellurium can reach 2%-30%. The primary crude tellurium, the secondary crude tellurium and the tertiary crude tellurium are then collected separately, and crude tellurium of different purity grades can be processed separately, thereby obtaining good economic benefits.
[0026] In an optional embodiment, after obtaining the tertiary filtrate, the following steps are also included: cadmium separation, adjusting the pH value of the tertiary filtrate to 8.5-10.5, adding a chemical precipitant, the reaction time is 20 minutes-40 minutes, then adding polyaluminum chloride and polyacrylamide, reacting for 5 minutes, and separating the precipitate to obtain a cadmium-containing precipitate and heavy metal-free wastewater.
[0027] Beneficial effect: After the recovery of tellurium is completed, cadmium is separated from the solution to obtain cadmium-containing precipitate, which is sold to cadmium recovery units. The heavy metal-free wastewater is no different from ordinary chemical wastewater because the two main polluting elements of tellurium and cadmium have been excluded. It can be directly put into the wastewater treatment pool for unified treatment.
[0028] In an optional embodiment, the chemical precipitant is sodium sulfide or a sodium phosphate solution with a concentration of 5%-15%, the concentration of polyaluminium chloride is 5%-15%, and the concentration of polyacrylamide is 0.1%.
[0029] Beneficial effects: By adding chemical precipitants, the precipitation of cadmium is promoted, making the separation of cadmium from the solution more thorough. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 A schematic diagram of a waste substrate treatment and recycling process of a method for treating waste substrates of a cadmium telluride photovoltaic module according to an embodiment of the present invention;
[0032] Figure 2 It is a schematic diagram of the overall process of a method for processing scrapped substrates of cadmium telluride photovoltaic modules according to an embodiment of the present invention;
[0033] Figure 3 A schematic diagram of a process for transferring substrate fragments between various devices in a method for processing scrapped substrates of cadmium telluride photovoltaic modules according to an embodiment of the present invention;
[0034] Figure 4 The present invention is a schematic flow chart of tellurium separation and cadmium separation in a method for processing a scrapped substrate of a cadmium telluride photovoltaic module according to an embodiment of the present invention. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0036] Combine the following Figures 1 to 4 , describing an embodiment of the present invention.
[0037] According to an embodiment of the present invention, a method for processing scrapped substrates of cadmium telluride photovoltaic modules is provided, comprising the following steps: crushing treatment, crushing the scrapped substrate to obtain substrate fragments; acid leaching treatment, mixing the substrate fragments with an acid leaching solution, stirring the reaction for a set time, separating the substrate fragments from the acid leaching solution to obtain pickled fragments, repeatedly using the acid leaching solution until it reaches a recycling standard, collecting the acid leaching solution to obtain collected acid leaching liquid; water washing treatment, washing the pickled fragments with water to obtain quasi-clean fragments, and collecting and storing the washing water; fragment drying, drying the quasi-clean fragments; fragment detection, performing heavy metal index detection on the dried quasi-clean fragments, completing the processing if the processing standard is met, and mixing the quasi-clean fragments with the substrate fragments to wait for re-acid leaching treatment if the processing standard is met.
[0038] In this embodiment, the scrapped substrates generated on the production line are easier to process more efficiently after being crushed. The substrate fragments are subjected to acid leaching treatment to separate the thin film containing cadmium and tellurium attached to the substrate fragments from the substrate, and then quasi-clean fragments are obtained after water washing. The quasi-clean fragments are tested. If they meet the treatment standards, that is, the cadmium residue and tellurium residue on the quasi-clean fragments are no longer hazardous waste standards, but are conventional waste products, they can be collected, stored and taken out as ordinary glass fragments. The storage and processing costs are low, effectively saving corporate costs. Since the main purpose of this method is to process scrapped substrates into quasi-clean fragments of conventional waste standards, rather than recycling cadmium or tellurium, it is suitable for small batches of scrapped substrates. The scrapped substrates can be processed in a timely manner, thereby effectively controlling the storage and pollution prevention costs of the production organization of cadmium telluride photovoltaic modules for storing scrapped substrates. In addition, the repeated use of the acid leaching solution can save material costs on the one hand, and on the other hand, it can enrich the cadmium or tellurium on the substrate fragments in the collected acid leaching solution, and then collect and store the collected acid leaching solution and cleaning water in a special container. Compared with the direct storage and pollution control of scrapped substrates, it is more convenient, with lower time and economic costs.
[0039] Specifically, the set time of the stirring reaction is related to the type and ratio of the acid leaching solution and the actual total amount of cadmium telluride film on the substrate fragments. In actual operation, the set time can be determined through sample experiments. In the process of drying the fragments, the quasi-cleaned fragments are separated from the water by drying or draining.
[0040] It should be noted that in the production process of cadmium telluride photovoltaic modules, scrapped substrates are collected through collection boxes, and then the scrapped substrates are transported to crushers and other equipment through lifting equipment such as belt elevators for crushing.
[0041] In one embodiment, during the crushing process, the scrapped substrate is crushed into particles with a size less than 2 CM.
[0042] Specifically, the scrapped substrate may be a whole substrate or a broken substrate. The scrapped substrate is broken once by a shredder and then put into a crusher for secondary crushing to obtain substrate fragments with smaller particle sizes.
[0043] In this embodiment, the scrapped substrates are crushed to obtain substrate fragments, and the particle size of the substrate fragments is controlled within 2CM by a sieve, which is convenient for storage and transportation, and also improves the efficiency of subsequent acid leaching, water washing and drying steps.
[0044] In one embodiment, when performing acid leaching treatment, the substrate fragments are placed in a drum reactor, and the substrate fragments are stirred when the drum of the drum reactor rotates in a first direction. When the drum of the drum reactor rotates in a second direction, the broken substrate is discharged from the discharge port of the drum reactor, and then the pickling fragments and the acid leaching liquid are separated by a spiral separator.
[0045] Specifically, the drum of the drum reactor has spiral blades in the drum, and the axis of the drum is arranged horizontally. When the drum rotates in a first direction, the blades stir the substrate fragments, and when the drum rotates in a second direction opposite to the first direction, the substrate fragments move toward the discharge port of the drum reactor driven by the blades, and when discharged, the substrate fragments and a small amount of acid leaching liquid are discharged. The feed trough of the spiral separator is arranged at the discharge port of the drum reactor, and is used to receive the acid leaching liquid and the substrate fragments.
[0046] In addition, specifically, there is also an acid leaching liquid in the feed tank of the spiral separator used for the acid leaching treatment, and the thin film on the surface of the substrate fragments continues to react with the oxidant in the acid leaching liquid after entering the spiral separator.
[0047] In this embodiment, a drum reactor is used instead of a reactor to perform acid leaching treatment on the substrate fragments, so that the substrate fragments in the reactor are prevented from accumulating and blocking the lower discharge port of the reactor. In addition, the drum reactor can be used to directly pour materials through the feed hopper to add materials. The drum reactor rotates in two directions to stir the substrate fragments and discharge the substrate fragments that have completed the acid leaching treatment from the drum. The operation is convenient, the material feeding and discharging are fast, and the efficiency is high. In addition, a spiral separator is used to separate the substrate fragments from the acid leaching liquid. The acid leaching liquid in the spiral separator can continue to separate the thin film on the surface of the substrate fragments. At the same time, the spiral separator gradually lifts the substrate fragments above the liquid level. As the substrate fragments are lifted, most of the acid leaching liquid attached to the surface of the substrate fragments flows back to the bottom of the spiral separator. It is convenient and quick, and reduces the difficulty of cleaning the pickled fragments. The spiral separator is not prone to blockage and jamming, and the separation efficiency of the substrate fragments is stable and reliable, which can make the substrate fragments output evenly.
[0048] In one embodiment, during the acid leaching treatment, the acid leaching liquid is sulfuric acid and hydrogen peroxide, wherein the concentration of sulfuric acid is 0.5 mol / L-8 mol / L, and the concentration of hydrogen peroxide is 5%-15%, or the acid leaching liquid is nitric acid, and the concentration of nitric acid is 30%-65%. During the acid leaching treatment, when the acid leaching liquid is sulfuric acid and hydrogen peroxide, the acid leaching liquid is heated to 40°C-85°C.
[0049] In this embodiment, the cadmium telluride film attached to the substrate fragments is corroded and oxidized by an acid immersion solution, so that the cadmium telluride film is separated from the substrate fragments.
[0050] In one embodiment, during the acid leaching treatment, the liquid-to-solid ratio of the acid leaching liquid to the substrate fragments is in a range of 3 L:1 kg to 10 L:1 kg, and the reaction time is 0.2 hours to 1 hour.
[0051] In this embodiment, the liquid-to-solid ratio and the reaction time are flexibly adjusted according to the amount of cadmium telluride film attached to the scrapped substrate during actual processing and the number of broken substrates to be processed, thereby further improving the processing efficiency and saving reagent costs.
[0052] In one embodiment, the collected acid extract is diluted 5 to 10 times and then mixed with the cleaning water and stored together.
[0053] In this embodiment, the collected acid leaching liquid is mixed with the cleaning water and stored together, which reduces the corrosiveness of the collected acid leaching liquid and facilitates storage. The acid washing liquid is mixed with the cleaning water after absorption to avoid a large amount of solid slag during the neutralization of the concentrated recovered acid solution, and the acid solution concentration in the reactor is high, and the amount of the dosing agent is not easy to control, which affects the reaction effect.
[0054] In one embodiment, the acid leaching solution is repeatedly used until the suspended matter in the acid leaching solution is greater than or equal to 30% to reach the recovery standard.
[0055] Specifically, during the acid leaching process, the acid leaching solution in both the drum reactor and the spiral separator will be consumed over time. Under normal circumstances, when the acid leaching solution is consumed to a certain extent, the staff only needs to add new acid leaching solution to the drum reactor and the spiral separator. This is not only simple to operate, but also allows the tellurium and cadmium components on the substrate fragments to be continuously enriched in the acid leaching solution. However, as the number of times some of the acid leaching solutions are reused increases, the overall oxidant ratio in the acid leaching solution will decrease, and the suspended matter will increase, requiring the acid leaching solution to be replaced.
[0056] In this embodiment, during the repeated use of the acid leaching solution, the cadmium telluride film is continuously enriched in the acid leaching solution. At this time, the concentration of the effective oxidant component in the acid leaching solution is reduced and the processing capacity is weakened. The acid leaching solution is recycled. On the one hand, the enriched cadmium and tellurium can be collected together. On the other hand, it is convenient to ensure the overall concentration of the effective oxidant component of the acid leaching solution in the reaction container when adding new acid leaching solution, thereby ensuring the processing efficiency and quality of the substrate fragments.
[0057] It should be noted that after the collected acid leaching liquid is recovered, the suspended matter in the acid leaching liquid can be filtered, and the waste residue from the filtration can be tested. If the tellurium content is greater than 1%, the waste residue is stored. After accumulating a certain amount, it is pickled and the tellurium is precipitated and collected. If the low content is less than or equal to 1%, the waste residue is directly sold to a hazardous waste treatment agency.
[0058] In one embodiment, the water washing treatment includes at least a primary water washing and a secondary water washing performed sequentially. A spiral separator is used to clean the pickled fragments during both the primary water washing and the secondary water washing. Clean water is input into the spiral separator 150 mm to 300 mm above the liquid level so that the clean water flows from the end of the spiral separator to the front end, and compressed air is delivered to the bottom of the spiral separator feed trough used in the primary water washing process.
[0059] Specifically, in order to make the pickled debris receive more thorough cleaning during the rising process in the water-washing spiral separator, the height of the clean water input position can be controlled between 200 mm and 300 mm.
[0060] In this embodiment, the pickled fragments are washed twice by arranging a primary water wash and a secondary water wash, so that the pickling liquid attached to the surface of the pickled fragments is cleaned. Since the pickled fragments are evenly lifted by the spiral separator, compressed air is delivered at the bottom of the feed tank of the spiral separator to stir the pickled fragments, so that the pickled fragments are quickly separated from the pickled liquid attached to the surface, and then clean water is input from a position near the end of the spiral separator to rinse the pickled fragments. The water flow carries the pickling liquid washed from the pickled fragments back to the feed tank, so that the pickled fragments are gradually cleaned along the ascending path, and then the pickled fragments are further rinsed by the spiral separator of the secondary water wash, so that most of the pickling liquid is separated from the pickled fragments, and then conventional glass debris waste that does not meet the hazardous waste standards is obtained, which is convenient for stacking and storing by a simple method, or directly sold to ordinary waste recycling units.
[0061] In one embodiment, when performing fragment detection, a quasi-clean fragment sample of no less than 2 kg is taken, and the quasi-clean fragment sample is oscillated and soaked in nitric acid with a pH less than 2 for 18 hours to 22 hours, and the liquid-to-solid ratio of nitric acid to the quasi-clean fragment sample is 10L:1kg. After the treatment, the total cadmium is tested. When the total cadmium is less than 1 mg / L, the quasi-clean fragment meets the treatment standard, otherwise it does not meet the treatment standard.
[0062] In this embodiment, the standard for hazardous waste is mainly the content of heavy metals in the waste. For scrapped substrates, it is mainly the content of cadmium. Therefore, the total cadmium index in the quasi-cleaning fragments is tested. If the standard is met, the quasi-cleaning fragments are not hazardous waste and can be directly sold out. If the standard is not met, the quasi-cleaning fragments have not been cleaned up and need to be reprocessed and tested again.
[0063] In one embodiment, after the collection of the acid leaching liquid is completed, the following steps are also included: tellurium separation, including pretreatment, putting the collected acid leaching liquid or cleaning water into a container, adjusting the pH value to 2-3, and then adjusting the voltage in the container to 350MV-650MV, reacting for 0.5 hours to 1.5 hours to obtain a tellurium recovery liquid; primary separation, adjusting the pH value of the tellurium recovery liquid to 2.5-3.5, filtering the precipitate to obtain primary crude tellurium and primary filtrate; secondary separation, adjusting the pH value of the primary filtrate to 3.5-4.5, filtering the precipitate to obtain secondary crude tellurium and secondary filtrate; tertiary separation, adjusting the pH value of the secondary filtrate to 4.5-6.5, filtering the precipitate to obtain tertiary crude tellurium and tertiary filtrate; crude tellurium collection, collecting the primary crude tellurium, the secondary crude tellurium and the tertiary crude tellurium respectively.
[0064] Specifically, the voltage in the liquid in the container is controlled by a redox potentiometer. The pH value is adjusted by adding caustic soda through an online pH controller. In the process of primary separation, after adjusting the pH value, the solution is filtered three times to obtain primary crude tellurium, and the primary filtrate is transferred to the reaction tank of secondary separation; in the process of secondary separation, after adjusting the pH value, the solution is filtered three times to obtain secondary crude tellurium, and the secondary filtrate is transferred to the reaction tank of tertiary separation; in the process of tertiary separation, after adjusting the pH value, the solution is filtered three times to obtain tertiary crude tellurium.
[0065] In this embodiment, by graded separation of crude tellurium at different pH values, tellurium and solution can be separated more thoroughly, and the tellurium content of primary crude tellurium can reach 40%-85%, the content of secondary crude tellurium can reach 20%-50%, and the content of tertiary crude tellurium can reach 2%-30%. The primary crude tellurium, secondary crude tellurium and tertiary crude tellurium are then collected separately, and crude tellurium of different purity grades can be processed separately, thereby obtaining good economic benefits.
[0066] In one embodiment, after obtaining the tertiary filtrate, the following steps are also included: cadmium separation, adjusting the pH value of the tertiary filtrate to 8.5-10.5, adding a chemical precipitant, the reaction time is 20 minutes-40 minutes, then adding polyaluminum chloride and polyacrylamide, reacting for 5 minutes, and separating the precipitate to obtain a cadmium-containing precipitate and heavy metal-free wastewater.
[0067] In this embodiment, after the recovery of tellurium is completed, cadmium is separated from the solution to obtain a cadmium-containing precipitate, which is sold to a cadmium recovery unit. The heavy metal-free wastewater is no different from ordinary chemical wastewater because the two main polluting elements, tellurium and cadmium, have been eliminated, and can be directly put into a wastewater treatment pool for unified treatment.
[0068] In one embodiment, the chemical precipitant is sodium sulfide or a sodium phosphate solution with a concentration of 5%-15%, the concentration of polyaluminium chloride is 5%-15%, and the concentration of polyacrylamide is 0.1%.
[0069] In this embodiment, the precipitation of cadmium element is promoted by adding a chemical precipitant, so that the cadmium and the solution are separated more thoroughly.
[0070] It should be noted that, in some of the above embodiments, if nitric acid is used as the acid leaching solution during the acid leaching process, after the cadmium separation is completed, the heavy metal-free wastewater is subjected to nitrate removal treatment, and ferrate or other oxidants are added to the heavy metal wastewater to convert the nitrite in the heavy metal-free wastewater into nitrate, and then the nitrate in the heavy metal-free wastewater is separated by a nitrate adsorption resin (A-62MP), and finally the heavy metal-free wastewater is discharged into a wastewater treatment pool.
[0071] Although the embodiments of the present invention have been described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.
Claims
1. A method for processing scrapped substrates of cadmium telluride photovoltaic modules, characterized in that: The following steps are involved: Crushing treatment, crushing the scrapped substrate to obtain substrate fragments; Acid leaching treatment, mixing the substrate fragments with an acid leaching solution, stirring the reaction for a set time, separating the substrate fragments from the acid leaching solution to obtain pickled fragments, repeatedly using the acid leaching solution until it reaches a recycling standard, and collecting and storing the acid leaching solution; Water washing treatment, washing the acid washed fragments with water to obtain quasi-clean fragments, and collecting and storing the washing water; Chip drying, drying the quasi-cleaned chips; Fragment detection: the quasi-cleaned fragments after drying are tested for heavy metal indicators. If they meet the treatment standards, the treatment is completed. If they do not meet the treatment standards, the quasi-cleaned fragments are mixed with the substrate fragments and wait for re-acid leaching treatment.
2. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 1, characterized in that: During the crushing process, the scrapped substrate is crushed into particles with a diameter less than 2 cm.
3. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 1, characterized in that: When the acid leaching treatment is carried out, the substrate fragments are placed in a drum reactor. When the drum of the drum reactor rotates in a first direction, the substrate fragments are stirred. When the drum of the drum reactor rotates in a second direction, the broken substrate is discharged from the discharge port of the drum reactor. The pickling fragments are then separated from the acid leaching liquid by a spiral separator.
4. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 1, characterized in that: When the acid leaching treatment is performed, the acid leaching solution is sulfuric acid and hydrogen peroxide, wherein the concentration of sulfuric acid is 0.5mol / L-8mol / L, and the concentration of hydrogen peroxide is 5%-15%; Alternatively, the acid leaching solution is nitric acid, and the concentration of the nitric acid is 30%-65%. During the acid leaching treatment, when the acid leaching solution is sulfuric acid and hydrogen peroxide, the acid leaching solution is heated to 40°C-85°C.
5. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 4, characterized in that: When the acid leaching treatment is performed, the liquid-to-solid ratio of the acid leaching liquid to the substrate fragments is in the range of 3L:1kg to 10L:1kg, and the reaction time is 0.2 hours to 1 hour.
6. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 1, characterized in that: The collected acid extract is diluted 5 to 10 times and then mixed with the cleaning water and stored together.
7. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 6, characterized in that: The acid leaching solution is repeatedly used until the suspended matter in the acid leaching solution is greater than or equal to 30% to reach the recovery standard.
8. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 1, characterized in that: The water washing treatment includes at least a primary water washing and a secondary water washing performed in sequence. A spiral separator is used to clean the pickled fragments during the primary water washing and the secondary water washing. Clean water is input into the spiral separator 150 mm to 300 mm above the liquid level so that the clean water flows from the end to the front end of the spiral separator. Compressed air is delivered to the bottom of the feed trough of the spiral separator used in the primary water washing process.
9. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 1, characterized in that: When conducting the fragment detection, take a quasi-clean fragment sample of no less than 2 kg, and oscillate and soak the quasi-clean fragment sample in nitric acid with a pH less than 2 for 18 hours to 22 hours. The liquid-to-solid ratio of nitric acid to the quasi-clean fragment sample is 10L:1kg. After the treatment, the total cadmium is tested. When the total cadmium is less than 1 mg / L, the quasi-clean fragment meets the treatment standard, otherwise it does not meet the treatment standard.
10. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to any one of claims 1 to 9, characterized in that: After the acid leaching liquid is collected, the following steps are also included: Tellurium separation, including pretreatment, putting the collected acid leaching solution or the cleaning water into a container, adjusting the pH value to 2-3, and then adjusting the voltage in the container to 350MV-650MV, reacting for 0.5 hour-1.5 hours, to obtain a tellurium recovery solution; Primary separation, adjusting the pH value of the tellurium recovery solution to 2.5-3.5, filtering the precipitate to obtain primary crude tellurium and primary filtrate; Secondary separation, adjusting the pH value of the primary filtrate to 3.5-4.5, filtering the precipitate to obtain secondary crude tellurium and secondary filtrate; Three-stage separation, adjusting the pH value of the secondary filtrate to 4.5-6.5, filtering the precipitate to obtain third-stage crude tellurium and third-stage filtrate; The crude tellurium is collected, and the primary crude tellurium, the secondary crude tellurium and the tertiary crude tellurium are collected respectively.
11. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 10, characterized in that: After obtaining the tertiary filtrate, the method further comprises the following steps: Cadmium separation, the pH value of the tertiary filtrate is adjusted to 8.5-10.5, and then a chemical precipitant is added, the reaction time is 20 minutes to 40 minutes, and then polyaluminum chloride and polyacrylamide are added, the reaction time is 5 minutes, and the precipitate is separated to obtain a cadmium-containing precipitate and heavy metal-free wastewater.
12. The method for processing scrapped substrates of cadmium telluride photovoltaic modules according to claim 11, characterized in that: The chemical precipitant is sodium sulfide or a sodium phosphate solution with a concentration of 5%-15%, the concentration of polyaluminium chloride is 5%-15%, and the concentration of polyacrylamide is 0.1%.
Citation Information
Patent Citations
Method for recovering tellurium and cadmium from cadmium telluride wastes
CN106277037A
Method of recovering tellurium from cadmium telluride waste materials
CN107128885A
Purification and recovery process of crude tellurium
CN112593245A
Method for enriching tellurium from platinum-palladium concentrate
CN112609089A
Recycling method of cadmium telluride waste assembly
CN113060707A