Method for preparing lithium carbonate from lepidolite

Through the sulfate roasting and extraction-carbon dioxide stripping process combined with resin degreasing and thermal centrifugal separation, the problems of high sodium carbonate consumption, low product yield and complex process during the extraction of lithium from lepidolite are solved, achieving high efficiency and low cost. Cost of lepidolite resource utilization.

CN118724028APending Publication Date: 2024-10-01SICHUAN ZHIYUAN LITHIUM IND CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202410760225.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing methods for extracting lithium from lepidolite have problems such as large consumption of sodium carbonate, low product yield, poor product quality, and complex processes.

Method used

The sulfate and lepidolite are mixed and roasted, and the leachate after impurity removal with pure water is used for extraction-carbon dioxide stripping process, combined with resin degreasing and thermal decomposition centrifugal separation, eliminating the need for sodium carbonate lithium precipitation and potassium ion efflux processes, simplifying the process process.

Benefits of technology

The process for extracting lithium from lepidolite is shortened, the product yield and quality are improved, the preparation cost is reduced, and the utilization value of lepidolite resources is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118724028A_ABST
    Figure CN118724028A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing lithium carbonate by utilizing lepidolite, which comprises the following steps: S1, mixing lepidolite with sulfate, and sequentially roasting, grinding, drying and countercurrent leaching to obtain lepidolite leachate; s2, mixing the lepidolite leachate with water according to a set proportion, and adding calcium hydroxide to obtain a mixed solution; s3, filtering calcium and magnesium ions in the mixed solution; s4, mixing the calcium and magnesium ion filtered mixed solution obtained in the step S3 with a lithium extraction organic extraction agent, and extracting to obtain a lithium-loaded extraction agent; s5, mixing the lithium-loaded extraction agent with water, and washing to obtain a clean lithium-loaded extraction agent; s6, combining the lithium-loaded extracting agent obtained in the step S5 with water and carbon dioxide, and then carrying out reverse extraction to obtain a lithium bicarbonate solution; and S7, the lithium bicarbonate solution is subjected to oil removal and calcium and magnesium ion removal with resin and then subjected to pyrolysis, and then pyrolysis liquid is subjected to centrifugal separation to obtain lithium carbonate. The method is simple in technological process and low in preparation cost, and the product yield and the product quality can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium extraction from lepidolite, in particular to a method for preparing lithium carbonate by utilizing lepidolite. Background Art

[0002] At present, the methods for extracting lithium from lithium mica mainly adopt lime roasting method, sulfate method and pressure cooking method. Among them, lime roasting method is to mix calcium oxide with lithium mica, roast it at high temperature, leach it with acid, and then obtain lithium hydroxide monohydrate through sedimentation, filtration, purification, impurity removal, evaporation, crystallization and drying process in sequence. This method has the problems of high energy consumption, large material flow and low lithium recovery rate. Pressure cooking method is to react lithium mica and sodium chloride in liquid phase under high pressure and high temperature conditions, and then obtain lithium carbonate through leaching, purification, evaporation and precipitation. The lithium mica material must be defluorinated first, which will cause environmental pollution and equipment corrosion problems, and the process route is long. Sulfate method is to mix lithium mica with auxiliary materials such as potassium sulfate, roast it at high temperature, ball mill, leach it, purify it, evaporate it, and precipitate it to prepare lithium carbonate. The impurity content of the leachate is high, the purification load is heavy, and the roasting process needs to use concentrated sulfuric acid as the raw material, which is highly corrosive. The above processes all consume a large amount of sodium carbonate in the lithium precipitation stage, resulting in low product yield and poor product quality. Potassium ions are enriched in the system and the mother liquor needs to be removed regularly, making the process complicated. Summary of the invention

[0003] The invention aims to solve the problems of large sodium carbonate consumption, low product yield, poor product quality and complicated process in the existing method for extracting lithium from lepidolite. A method for preparing lithium carbonate from lepidolite is provided. The method comprises the following steps: mixing sulfate with lepidolite and roasting the lepidolite, leaching and removing impurities from the roasted lepidolite with pure water, obtaining a lithium bicarbonate solution from the leached solution after impurity removal by an extraction-carbon dioxide stripping process, and then performing pyrolysis and centrifugal separation after oil removal and calcium and magnesium removal by resin to obtain lithium carbonate. When the invention is applied, sodium carbonate is no longer used to precipitate lithium when not feeding for the first time, and the process of potassium excretion is omitted, thereby shortening the lithium and sodium-potassium separation process at the rear end of lithium extraction from lepidolite. The process is simple and easy to implement, with low preparation cost, and can improve product yield and product quality.

[0004] The purpose of the present invention is mainly achieved through the following technical solutions:

[0005] A method for preparing lithium carbonate using lepidolite comprises the following steps:

[0006] Step S1, mixing lepidolite with sulfate, and sequentially performing roasting, grinding, drying, and countercurrent leaching to obtain a lepidolite leachate containing 10 to 30 g / L of lithium oxide;

[0007] Step S2, mixing the lepidolite leachate with water in a set ratio to obtain a composite raw material, and adding calcium hydroxide to the composite raw material to obtain a mixed solution with a hydroxide concentration of 0.1 to 0.5 mol / L;

[0008] Step S3, filtering the calcium and magnesium ions in the mixed solution obtained in step S2;

[0009] Step S4, mixing the mixed solution of filtered calcium and magnesium ions obtained in step S3 with a lithium-extracting organic extractant at a volume ratio of 1:3-10, and then extracting to obtain a lithium-loaded extractant;

[0010] Step S5, mixing the lithium-loaded extractant with water at a volume ratio of 10 to 30:1, and washing to obtain a clean lithium-loaded extractant;

[0011] Step S6, mixing the loaded lithium extractant obtained in step S5 with water and carbon dioxide in a volume ratio of 2:1 to 20:1, and then performing stripping to obtain a lithium bicarbonate solution;

[0012] Step S7, using resin to remove oil and calcium and magnesium ions from the lithium bicarbonate solution, followed by pyrolysis, and then centrifuging the pyrolysis solution to obtain lithium carbonate.

[0013] The calcium hydroxide added in step S2 of the present invention is prepared by mixing quicklime and water in a mass ratio of 1:3 to 5, the volume ratio of the leaching solution to the calcium hydroxide solution is 1:1 to 4, and 0.5 mol / L is the upper limit of the free hydroxide provided by calcium hydroxide. In step S4 of the present invention, the mixed solution is mixed with a lithium-extracting organic extractant in a mixing and settling tank, and in step S5, the lithium-loaded extractant is mixed with water and water in a mixing and settling tank. In step S6, the loaded lithium extractant is mixed with water and carbon dioxide in a volume ratio of 2:1 to 20:1 and then stripped in a stripping tower. In step S7, pyrolysis and centrifugation are carried out in a pyrolysis centrifugal kettle. The mixing and settling tank, stripping tower and pyrolysis centrifugal kettle are all based on the existing technology and are not repeated here. In step S3 of the present invention, the filtration is carried out by a plate and frame filter press, and the plate and frame filter press is based on the existing technology and is not repeated here. In order to make the leaching yield higher and the leaching more sufficient, the grinding mesh number in step S1 of the present invention is set to the range of 50 to 200 meshes. The lithium in the leaching solution obtained in step S1 exists in the form of lithium ions. Lithium is usually extracted from ore in terms of lithium oxide, corresponding to a lithium ion concentration of 5 to 15 g / l. The concentration of lithium oxide is controlled by controlling the leaching stage. In step S7 of this embodiment, lithium bicarbonate is converted into lithium carbonate by pyrolysis.

[0014] Furthermore, the sulfate used in step S1 is a mixture of calcium sulfate and sodium sulfate, and calcium carbonate is also added in step S1 to mix with lepidolite and sulfate; in step S1, lepidolite, calcium sulfate, calcium carbonate and sodium sulfate are mixed in a mass ratio of 60-65:20-25:5-10:5-10.

[0015] Furthermore, the calcination temperature in step S1 is 800-1000°C and the calcination time is 30-45 minutes. In the present invention, the lepidolite is heated at 800-1000°C for 30-45 minutes into a molten state to exchange lithium in the lepidolite.

[0016] Furthermore, when filtering calcium and magnesium ions in the mixed solution obtained in step S2 in step S3, free calcium ions are firstly removed by precipitation and filtration of the filtrate containing carbonate ions, and then sodium hydroxide is added to adjust the hydroxide concentration to 0.5-2 mol / L, and then the calcium and magnesium ions are removed by resin.

[0017] Furthermore, the organic extractant for lithium extraction used in step S4 is a ketone compound extractant and / or a phosphorus oxide compound extractant.

[0018] Furthermore, the raffinate obtained by extraction in step S4 is discharged after oil removal by resin, wherein the discharged raffinate is returned to the extraction process, so that resources can be better recycled.

[0019] Furthermore, when the lepidolite leachate is mixed with water in step S2, if it is the first feeding, the volume ratio of the lepidolite leachate to water is 1:1; if it is not the first feeding, when the lepidolite leachate is mixed with water in step S2, the raffinate discharged in step S4 is also added, and the volume ratio of the lepidolite leachate, the raffinate and the water is 2-4:3-6:1-2. The raffinate can be reused multiple times to increase the sodium-potassium concentration to prepare a double salt, which can be used for front-end roasting.

[0020] Further, the step S7 also includes cooling the centrifuged mother liquor to room temperature and then stripping to obtain a centrifuged mother liquor with a sodium ion concentration and a potassium ion concentration greater than 8g / L; when filtering the calcium and magnesium ions in the mixed solution obtained in step S2 in the step S3, if it is the first feeding, the filtrate uses the carbonate precipitation in the sodium carbonate solution to filter out free calcium ions, and if it is not the first feeding, the filtrate uses the carbonate precipitation in the centrifuged mother liquor treated in step S7 to filter out free calcium ions. The present invention adjusts the hydroxide concentration to 0.1-0.5mol / L, and then filters once with a plate and frame filter press, and the plate and frame filtrate uses the carbonate precipitation in the centrifuged mother liquor to remove free calcium ions (sodium carbonate is used instead of the centrifuged mother liquor in the initial feeding), and then sodium hydroxide is added to adjust the hydroxide concentration to 0.5-2mol / L, and the plate and frame filter press is used to filter again to obtain a calcium-magnesium-removed raw material, and then the calcium-removed magnesium resin is refined and decalcified to obtain a refined raw material. In this way, the present invention can prevent excessive calcium ions from affecting lithium extraction efficiency and lithium carbonate quality.

[0021] Furthermore, in step S7, the pyrolysis is performed at a temperature of 80 to 110° C. for 1 to 2.5 hours.

[0022] Furthermore, in step S7, the resin oil removal is carried out in an oil removal resin column, and the calcium and magnesium ion removal is carried out in a calcium and magnesium ion removal resin column; the method also includes an oil removal resin regeneration step and a calcium and magnesium removal resin regeneration step, and the oil removal resin regeneration step includes:

[0023] Step 11, using 0.3Mpa compressed air to uniformly pass in and out from the top of the degreasing resin column, with a total amount of 5BV and a passing time of 0.2h to discharge the residual liquid in the degreasing resin column;

[0024] Step 12, water is introduced into the degreasing resin column from the bottom to the top at a uniform speed, the introduction amount is 8 BV, and the introduction time is 0.2 h to clean the surface of the degreasing resin column;

[0025] Step 13, use 0.3Mpa compressed air to uniformly pass in and out from the top of the degreasing resin column, with a total amount of 5BV and a time of 0.2 to discharge the backwash water in the degreasing resin column;

[0026] Step 14, a 5% NaOH solution is uniformly introduced into the degreasing resin column, with a total amount of 1 BV and an introduction time of 2.5 h to saponify the extractant in the degreasing resin column and separate it from the resin;

[0027] Step 15, using 0.3Mpa compressed air to uniformly pass in and out from the top of the degreasing resin column, with a total amount of 5BV and a passing time of 0.2h to discharge the residual alkali solution in the resin column;

[0028] Step 16, water is introduced into the resin column at a uniform rate, with an introduction volume of 8 BV and an introduction time of 3 hours to wash away the residual alkali solution;

[0029] Step 17, using 0.3Mpa compressed air to enter and exit from the degreasing resin column, with a total amount of 5BV and a time of 0.2h to discharge the residual washing water in the resin column;

[0030] The calcium-magnesium-removal resin regeneration step comprises:

[0031] Step 21, using 0.3Mpa compressed air to uniformly pass in and out from the top of the calcium-magnesium resin column, the total amount of air passed is 5BV, the time of passing is 0.2h, and the residual liquid in the calcium-magnesium resin column is discharged;

[0032] Step 22, pure water is introduced into the calcium-magnesium removal resin column from the bottom to the top at a uniform speed, the introduction amount is 8 BV, and the introduction time is 0.2 h to clean the surface of the calcium-magnesium removal resin column;

[0033] Step 23, using 0.3Mpa compressed air to uniformly pass through the calcium and magnesium removal resin column from top to bottom, with a total amount of 5BV and a time of 0.2h to discharge the residual washing water in the resin column;

[0034] Step 24, using a 1% dilute sulfuric acid solution to uniformly pass through the calcium and magnesium removal resin column, with a total amount of 10BV passed through for 1 hour, and using the hydrogen ions in the sulfuric acid to exchange the calcium and magnesium ions in the resin; using a 5% dilute sulfuric acid solution to pass through the resin column, with a total amount of 1BV passed through for 1 hour, so that the calcium and magnesium ions in the resin of the calcium and magnesium removal resin column are completely replaced;

[0035] Step 25, using 0.3Mpa compressed air to uniformly pass through the calcium and magnesium removal resin column from top to bottom, with a total amount of 5BV and a time of 0.2h to discharge the residual acid in the resin column;

[0036] Step 26, water is introduced into the resin column at a uniform speed, with an introduction volume of 8 BV and an introduction time of 3 hours, to clean the residual acid on the surface of the calcium and magnesium resin column;

[0037] Step 27, use 0.3Mpa compressed air to uniformly pass in and out from the top of the calcium and magnesium removal resin column, with a total amount of 5BV and a passing time of 0.2h to discharge the residual washing water in the resin column.

[0038] In summary, the present invention has the following beneficial effects compared with the prior art: (1) The present invention uses lithium mica as a raw material, adopts sulfate mixed roasting of lithium mica, uses water to leach and remove impurities from the roasted lithium mica, and adopts extraction-carbon dioxide stripping process to extract the impurities from the leachate, which greatly shortens the process of preparing lithium carbonate using lithium mica as a raw material.

[0039] (2) The present invention proposes an extraction-carbon dioxide stripping process, which shortens the lithium and sodium-potassium separation process at the back end of lithium extraction from lepidolite. The centrifuged mother liquor can be recycled, and sodium carbonate is no longer used to precipitate lithium when not feeding for the first time.

[0040] (3) In the front-end extraction process of the present invention, the extractant only extracts lithium, and the sodium and potassium ions are discharged with the raffinate, thereby eliminating the process of regularly discharging potassium and improving the product yield and product quality.

[0041] (4) The preparation cost of the present invention is greatly reduced. At the same time, the present invention improves the utilization value of lithium mica resources and has a good industrialization prospect.

[0042] (5) The present invention can recycle the raffinate and the centrifugal mother liquor, so that the cost of the present invention can be further reduced when applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] The drawings described herein are used to provide a further understanding of the embodiments of the present invention, constitute a part of this application, and do not constitute a limitation of the embodiments of the present invention. In the drawings:

[0044] Figure 1The flowchart of a specific embodiment of the present invention is shown in FIG. DETAILED DESCRIPTION

[0045] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0046] Embodiment 1:

[0047] like Figure 1 As shown, a method for preparing lithium carbonate using lepidolite comprises the following steps: step S1, mixing lepidolite with sulfate, and sequentially performing roasting, grinding, drying, and countercurrent leaching to obtain a lepidolite leachate containing 10 g / L of lithium oxide; step S2, mixing the lepidolite leachate with water according to a set ratio to obtain a composite raw material, and adding calcium hydroxide to the composite raw material to obtain a mixed solution with a hydroxide concentration of 0.1 mol / L; step S3, filtering calcium and magnesium ions in the mixed solution obtained in step S2; step S4, filtering the filtered calcium obtained in step S3 The mixed solution of magnesium ions is mixed with an organic extractant for lithium extraction at a volume ratio of 1:8, and then extracted to obtain an extractant loaded with lithium; step S5, the extractant loaded with lithium is mixed with water at a volume ratio of 25:1, and washed to obtain a clean extractant loaded with lithium; step S6, the lithium extractant loaded with lithium obtained in step S5 is mixed with water and carbon dioxide at a volume ratio of 2:10:1, and then stripped to obtain a lithium bicarbonate solution; step S7, the lithium bicarbonate solution is degreased with resin and calcium and magnesium ions are removed, and then the pyrolysis liquid is centrifuged to obtain lithium carbonate. Among them, the sulfate used in step S1 is a sulfate mixed with calcium sulfate and sodium sulfate, and calcium carbonate is also added in step S1 to mix with lithium mica and sulfate; in step S1, lithium mica, calcium sulfate, calcium carbonate and sodium sulfate are mixed at a mass ratio of 65:20:5:10. In step S1, the roasting temperature is 1000°C and the roasting time is 30 minutes.

[0048] In step S3 of this embodiment, when filtering the calcium and magnesium ions in the mixed solution obtained in step S2, first use the filtrate with carbonate ions to precipitate and filter out the free calcium ions, then add sodium hydroxide to adjust the hydroxide concentration to 0.5 mol / L, and then use resin to remove the calcium and magnesium ions. The organic extractant for lithium extraction used in step S4 of this embodiment uses a ketone compound extractant and / or a phosphorus oxide compound extractant. In this embodiment, the organic extractant for lithium extraction specifically uses LIX54-100 and Cyanex923 mixed in a volume ratio of 1:1. The raffinate obtained by extraction in step S4 is discharged after oil removal by resin. When mixing the lithium mica leachate with water in step S2, if it is the first feeding, the volume ratio of the lithium mica leachate to water is 1:1; if it is not the first feeding, when mixing the lithium mica leachate with water in step S2, the raffinate discharged in step S4 is also added, and the volume ratio of the lithium mica leachate, the raffinate and water is 3:6:1.

[0049] In this embodiment, step S7 further includes cooling the centrifugal mother liquor obtained by centrifugation to room temperature and then stripping to obtain a centrifugal mother liquor having a sodium ion concentration and a potassium ion concentration greater than 8 g / L; when filtering the calcium and magnesium ions in the mixed solution obtained in step S2 in step S3, if it is the first feeding, the filtrate is filtered out by carbonate precipitation in the sodium carbonate solution to remove free calcium ions, and if it is not the first feeding, the filtrate is filtered out by carbonate precipitation in the centrifugal mother liquor treated in step S7 to remove free calcium ions. In step S7, the pyrolysis is performed at a temperature of 110° C. for 1 hour.

[0050] In step S7 of this embodiment, the resin is deoiled in the deoiling resin column, and the calcium and magnesium ion removal is carried out in the calcium and magnesium ion removal resin column. This embodiment also includes a deoiling resin regeneration step and a calcium and magnesium resin regeneration step, and the deoiling resin regeneration step includes: step 11, using 0.3Mpa compressed air to uniformly pass in and out from the top of the deoiling resin column, the total amount of which is 5BV, and the time of passing is 0.2h to discharge the residual liquid in the deoiling resin column; step 12, water is uniformly passed in and out from the bottom of the deoiling resin column, the amount of which is 8BV, and the time of passing is 0.2h to clean the surface of the deoiling resin column; step 13, using 0.3Mpa compressed air to uniformly pass in and out from the top of the deoiling resin column, the total amount of which is 5BV, and the time of passing is 0.2h to discharge the backwash water in the deoiling resin column; step 14, using a concentration of 5% NaOH solution is uniformly introduced into and out of the degreasing resin column, with a total amount of 1BV and an introduction time of 2.5h, to saponify the extractant in the degreasing resin column and separate it from the resin; step 15, 0.3Mpa compressed air is uniformly introduced into and out of the degreasing resin column, with a total amount of 5BV and an introduction time of 0.2h, to discharge the residual alkali solution in the resin column; step 16, water is uniformly introduced into and out of the resin column, with an introduction amount of 8BV and an introduction time of 3h, to rinse the residual alkali solution; step 17, 0.3Mpa compressed air is introduced into and out of the degreasing resin column, with a total amount of 5BV and an introduction time of 0.2h, to discharge the residual washing water in the resin column.The regeneration steps of the calcium removal magnesium resin of the present embodiment include: step 21, using 0.3Mpa compressed air to uniformly pass in and out from the top of the calcium removal magnesium resin column, the total amount of which is 5BV, and the time of passing is 0.2h, and the residual liquid in the calcium removal magnesium resin column is discharged; step 22, pure water is uniformly passed in and out from the bottom of the calcium removal magnesium resin column, the amount of which is 8BV, and the time of passing is 0.2h to clean the surface of the calcium removal magnesium resin column; step 23, using 0.3Mpa compressed air to uniformly pass in and out from the top of the calcium removal magnesium resin column, the total amount of which is 5BV, and the time of passing is 0.2h, and the residual wash water in the resin column is discharged; step 24, using a 1% dilute sulfuric acid solution to uniformly pass in and out from the top of the calcium removal magnesium resin column, the total amount of which is 10BV, and the time of passing is 1h, and sulfur is used to remove the residual water from the resin column. The hydrogen ions in the acid are exchanged with the calcium and magnesium ions in the resin; a 5% dilute sulfuric acid solution is used to enter and exit the resin column, with a total amount of 1BV and an entry time of 1h, so that the calcium and magnesium ions in the resin of the calcium and magnesium removal resin column are completely replaced; step 25, 0.3Mpa compressed air is used to enter and exit the calcium and magnesium removal resin column at a uniform speed, with a total amount of 5BV and an entry time of 0.2h, and the residual acid in the resin column is discharged; step 26, water is passed from the resin column at a uniform speed, with an entry amount of 8BV and an entry time of 3h to clean the residual acid on the surface of the calcium and magnesium removal resin column; step 27, 0.3Mpa compressed air is used to enter and exit the calcium and magnesium removal resin column at a uniform speed, with a total amount of 5BV and an entry time of 0.2h, and the residual washing water in the resin column is discharged. Wherein, the oil removal resin of this embodiment preferably adopts a macroporous adsorption resin, and the calcium and magnesium removal resin preferably adopts an amino acid type chelating resin.

[0051] After testing, the purity of the lithium carbonate prepared by the method of this embodiment is 99.6%.

[0052] Embodiment 2:

[0053] A method for preparing lithium carbonate using lepidolite comprises the following steps: step S1, mixing lepidolite with sulfate, and sequentially performing roasting, grinding, drying, and countercurrent leaching to obtain a lepidolite leachate containing 20 g / L of lithium oxide; step S2, mixing the lepidolite leachate with water according to a set ratio to obtain a composite raw material, and adding calcium hydroxide to the composite raw material to obtain a mixed solution with a hydroxide concentration of 0.2 mol / L; step S3, filtering calcium and magnesium ions in the mixed solution obtained in step S2; step S4, filtering the filtered calcium and magnesium ions obtained in step S3 The mixed solution of the seeds is mixed with a lithium-extracting organic extractant in a volume ratio of 1:23, and then extracted to obtain a lithium-loaded extractant; step S5, the lithium-loaded extractant is mixed with water in a volume ratio of 15:1, and washed to obtain a clean lithium-loaded extractant; step S6, the lithium-loaded extractant obtained in step S5 is mixed with water and carbon dioxide in a volume ratio of 2:1:1, and then stripped to obtain a lithium bicarbonate solution; step S7, the lithium bicarbonate solution is degreased with resin and calcium and magnesium ions are removed, and then the pyrolysis liquid is centrifuged to obtain lithium carbonate. Among them, the sulfate used in step S1 is a sulfate mixed with calcium sulfate and sodium sulfate, and calcium carbonate is also added in step S1 to mix with lithium mica and sulfate; in step S1, lithium mica, calcium sulfate, calcium carbonate and sodium sulfate are mixed in a mass ratio of 63:25:8:5. In step S1, the roasting temperature is 900°C and the roasting time is 40min.

[0054] In step S3 of this embodiment, when filtering the calcium and magnesium ions in the mixed solution obtained in step S2, first use the filtrate with carbonate ions to precipitate and filter out the free calcium ions, then add sodium hydroxide to adjust the hydroxide concentration to 1.2 mol / L, and then use resin to remove the calcium and magnesium ions. The organic extractant for lithium extraction used in step S4 of this embodiment uses a ketone compound extractant and / or a phosphorus oxide compound extractant. In this embodiment, the organic extractant for lithium extraction specifically uses LIX54 and Cyanex923 mixed in a volume ratio of 1:1. The raffinate obtained by extraction in step S4 is discharged after oil removal by resin. When mixing the lithium mica leachate with water in step S2, if it is the first feeding, the volume ratio of the lithium mica leachate to water is 1:1; if it is not the first feeding, when mixing the lithium mica leachate with water in step S2, the raffinate discharged in step S4 is also added, and the volume ratio of the lithium mica leachate, the raffinate and water is 4:3:1.5.

[0055] In this embodiment, step S7 further includes cooling the centrifugal mother liquor obtained by centrifugation to room temperature and then stripping to obtain a centrifugal mother liquor having a sodium ion concentration and a potassium ion concentration greater than 8 g / L; when filtering the calcium and magnesium ions in the mixed solution obtained in step S2 in step S3, if it is the first feeding, the filtrate is filtered out by carbonate precipitation in the sodium carbonate solution to remove free calcium ions, and if it is not the first feeding, the filtrate is filtered out by carbonate precipitation in the centrifugal mother liquor treated in step S7 to remove free calcium ions. In step S7, the pyrolysis is performed at 95° C. for 1.8 hours.

[0056] In step S7 of this embodiment, the resin oil removal is carried out in the oil removal resin column, and the calcium and magnesium ion removal is carried out in the calcium and magnesium ion removal resin column. The oil removal resin regeneration step and the calcium and magnesium removal resin regeneration step of this embodiment are the same as those of embodiment 1, and will not be repeated here.

[0057] After testing, the purity of the lithium carbonate prepared by the method of this embodiment is 99.5%.

[0058] Embodiment 3:

[0059] A method for preparing lithium carbonate using lepidolite comprises the following steps: step S1, mixing lepidolite with sulfate, and sequentially performing roasting, grinding, drying, and countercurrent leaching to obtain a lepidolite leachate containing 30 g / L of lithium oxide; step S2, mixing the lepidolite leachate with water according to a set ratio to obtain a composite raw material, and adding calcium hydroxide to the composite raw material to obtain a mixed solution with a hydroxide concentration of 0.15 mol / L; step S3, filtering calcium and magnesium ions in the mixed solution obtained in step S2; step S4, filtering the filtered calcium and magnesium ions obtained in step S3 The mixed solution of ions is mixed with a lithium-extracting organic extractant at a volume ratio of 1:3, and then extracted to obtain a lithium-loaded extractant; step S5, the lithium-loaded extractant is mixed with water at a volume ratio of 30:1, and washed to obtain a clean lithium-loaded extractant; step S6, the lithium-loaded extractant obtained in step S5 is mixed with water and carbon dioxide at a volume ratio of 2:20:1, and then stripped to obtain a lithium bicarbonate solution; step S7, the lithium bicarbonate solution is degreased with resin and calcium and magnesium ions are removed, and then the pyrolysis liquid is centrifuged to obtain lithium carbonate. Among them, the sulfate used in step S1 is a sulfate mixed with calcium sulfate and sodium sulfate, and calcium carbonate is also added in step S1 to mix with lithium mica and sulfate; in step S1, lithium mica, calcium sulfate, calcium carbonate and sodium sulfate are mixed at a mass ratio of 60:23:10:8. In step S1, the roasting temperature is 800°C and the roasting time is 45 minutes.

[0060] In step S3 of this embodiment, when filtering the calcium and magnesium ions in the mixed solution obtained in step S2, first use the filtrate with carbonate ions to precipitate and filter out the free calcium ions, then add sodium hydroxide to adjust the hydroxide concentration to 2 mol / L, and then use resin to remove the calcium and magnesium ions. The organic extractant for lithium extraction used in step S4 of this embodiment uses a ketone compound extractant and / or a phosphorus oxide compound extractant. In this embodiment, the organic extractant for lithium extraction specifically uses LIX54 and TRPO mixed in a volume ratio of 1:1. The raffinate obtained by extraction in step S4 is discharged after oil removal by resin. When mixing the lithium mica leachate with water in step S2, if it is the first feeding, the volume ratio of the lithium mica leachate to water is 1:1; if it is not the first feeding, when mixing the lithium mica leachate with water in step S2, the raffinate discharged in step S4 is also added, and the volume ratio of the lithium mica leachate, the raffinate and water is 2:5:2.

[0061] In this embodiment, step S7 further includes cooling the centrifugal mother liquor obtained by centrifugation to room temperature and then stripping to obtain a centrifugal mother liquor having a sodium ion concentration and a potassium ion concentration greater than 8 g / L; when filtering the calcium and magnesium ions in the mixed solution obtained in step S2 in step S3, if it is the first feeding, the filtrate is filtered out by carbonate precipitation in the sodium carbonate solution to remove free calcium ions, and if it is not the first feeding, the filtrate is filtered out by carbonate precipitation in the centrifugal mother liquor treated in step S7 to remove free calcium ions. In step S7, the pyrolysis is performed at 80° C. for 2.5 hours.

[0062] In step S7 of this embodiment, the resin oil removal is carried out in the oil removal resin column, and the calcium and magnesium ion removal is carried out in the calcium and magnesium ion removal resin column. The oil removal resin regeneration step and the calcium and magnesium removal resin regeneration step of this embodiment are the same as those of embodiment 1, and will not be repeated here.

[0063] After testing, the purity of the lithium carbonate prepared by the method of this embodiment is 99.4%.

[0064] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing lithium carbonate using lepidolite, characterized in that: The following steps are involved: Step S1, mixing lepidolite with sulfate, and sequentially performing roasting, grinding, drying, and countercurrent leaching to obtain a lepidolite leachate containing 10 to 30 g / L of lithium oxide; Step S2, mixing the lepidolite leachate with water in a set ratio to obtain a composite raw material, and adding calcium hydroxide to the composite raw material to obtain a mixed solution with a hydroxide concentration of 0.1 to 0.5 mol / L; Step S3, filtering the calcium and magnesium ions in the mixed solution obtained in step S2; Step S4, mixing the mixed solution of filtered calcium and magnesium ions obtained in step S3 with a lithium-extracting organic extractant at a volume ratio of 1:3-10, and then extracting to obtain a lithium-loaded extractant; Step S5, mixing the lithium-loaded extractant with water at a volume ratio of 10 to 30:1, and washing to obtain a clean lithium-loaded extractant; Step S6, mixing the loaded lithium extractant obtained in step S5 with water and carbon dioxide in a volume ratio of 2:1 to 20:1, and then performing stripping to obtain a lithium bicarbonate solution; Step S7, using resin to remove oil and calcium and magnesium ions from the lithium bicarbonate solution, followed by pyrolysis, and then centrifuging the pyrolysis solution to obtain lithium carbonate.

2. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: The sulfate used in step S1 is a mixture of calcium sulfate and sodium sulfate. Calcium carbonate is also added in step S1 to mix with lepidolite and sulfate. In step S1, lepidolite, calcium sulfate, calcium carbonate and sodium sulfate are mixed in a mass ratio of 60-65:20-25:5-10:5-10.

3. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: In step S1, the calcination temperature is 800-1000° C., and the calcination time is 30-45 minutes.

4. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: When filtering calcium and magnesium ions in the mixed solution obtained in step S2 in step S3, firstly use the filtrate with carbonate ions to precipitate and filter out free calcium ions, then add sodium hydroxide to adjust the hydroxide concentration to 0.5-2 mol / L, and then use resin to remove calcium and magnesium ions.

5. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: The organic extractant for lithium extraction used in step S4 is a ketone compound extractant and / or a phosphorus oxide compound extractant.

6. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: The raffinate obtained by extraction in step S4 is discharged after oil removal by resin.

7. A method for preparing lithium carbonate using lepidolite according to claim 6, characterized in that: When the lepidolite leachate is mixed with water in step S2, if it is the first time to feed, the volume ratio of the lepidolite leachate to water is 1:1; if it is not the first time to feed, when the lepidolite leachate is mixed with water in step S2, the raffinate discharged in step S4 is also added, and the volume ratio of the lepidolite leachate, the raffinate and the water is 2-4:3-6:1-2.

8. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: The step S7 further comprises cooling the centrifuged mother liquor obtained by centrifugation to room temperature and then performing back extraction to obtain a centrifuged mother liquor having a sodium ion concentration and a potassium ion concentration both greater than 8 g / L; when filtering the calcium and magnesium ions in the mixed liquor obtained in the step S2 in the step S3, if it is the first feeding, the filtrate is filtered out by using carbonate precipitates in the sodium carbonate solution to remove free calcium ions; if it is not the first feeding, the filtrate is filtered out by using carbonate precipitates in the centrifuged mother liquor treated in step S7 to remove free calcium ions.

9. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: In step S7, the pyrolysis is performed at a temperature of 80 to 110° C. for 1 to 2.5 hours.

10. A method for preparing lithium carbonate using lepidolite according to claim 1, characterized in that: In step S7, the resin is deoiled in an oil-removing resin column, and the calcium and magnesium ion removal is carried out in a calcium and magnesium ion removal resin column; the method also includes an oil-removing resin regeneration step and a calcium and magnesium removal resin regeneration step, and the oil-removing resin regeneration step includes: Step 11, using 0.3Mpa compressed air to uniformly pass in and out from the top of the degreasing resin column, with a total amount of 5BV and a passing time of 0.2h to discharge the residual liquid in the degreasing resin column; Step 12, water is introduced into the degreasing resin column from the bottom to the top at a uniform speed, the introduction amount is 8 BV, and the introduction time is 0.2 h to clean the surface of the degreasing resin column; Step 13, use 0.3Mpa compressed air to uniformly pass in and out from the top of the degreasing resin column, with a total amount of 5BV and a time of 0.2 to discharge the backwash water in the degreasing resin column; Step 14, a 5% NaOH solution is uniformly introduced into the degreasing resin column, with a total amount of 1 BV and an introduction time of 2.5 h to saponify the extractant in the degreasing resin column and separate it from the resin; Step 15, using 0.3Mpa compressed air to uniformly pass in and out from the top of the degreasing resin column, with a total amount of 5BV and a passing time of 0.2h to discharge the residual alkali solution in the resin column; Step 16, water is introduced into the resin column at a uniform rate, with an introduction volume of 8 BV and an introduction time of 3 hours to wash away the residual alkali solution; Step 17, using 0.3Mpa compressed air to enter and exit from the degreasing resin column, with a total amount of 5BV and a time of 0.2h to discharge the residual washing water in the resin column; The calcium-magnesium-removal resin regeneration step comprises: Step 21, using 0.3Mpa compressed air to uniformly pass in and out from the top of the calcium-magnesium resin column, the total amount of air passed is 5BV, the time of passing is 0.2h, and the residual liquid in the calcium-magnesium resin column is discharged; Step 22, pure water is introduced into the calcium-magnesium removal resin column from the bottom to the top at a uniform speed, the introduction amount is 8 BV, and the introduction time is 0.2 h to clean the surface of the calcium-magnesium removal resin column; Step 23, using 0.3Mpa compressed air to uniformly pass through the calcium and magnesium removal resin column from top to bottom, with a total amount of 5BV and a time of 0.2h to discharge the residual washing water in the resin column; Step 24, using a 2% dilute sulfuric acid solution to uniformly pass through the calcium and magnesium removal resin column, with a total amount of 10BV passed through for 1 hour, and using the hydrogen ions in the sulfuric acid to exchange the calcium and magnesium ions in the resin; using a 5% dilute sulfuric acid solution to pass through the resin column, with a total amount of 1BV passed through for 1 hour, so that the calcium and magnesium ions in the resin of the calcium and magnesium removal resin column are completely replaced; Step 25, using 0.3Mpa compressed air to uniformly pass through the calcium and magnesium removal resin column from top to bottom, with a total amount of 5BV and a time of 0.2h to discharge the residual acid in the resin column; Step 26, water is introduced into the resin column at a uniform speed, with an introduction volume of 8 BV and an introduction time of 3 hours, to clean the residual acid on the surface of the calcium and magnesium resin column; Step 27, use 0.3Mpa compressed air to uniformly pass in and out from the top of the calcium and magnesium removal resin column, with a total amount of 5BV and a passing time of 0.2h to discharge the residual washing water in the resin column.

Citation Information

Cited By

  • Preparation method of high-purity lithium fluoride

    CN119240753A

  • Method for recovering lithium, rubidium and cesium elements in lepidolite

    CN119800100A

  • Method for recovering lithium, rubidium and cesium elements from lepidolite

    CN119800100B