Mn (II)-based metal halide scintillator material and preparation method and application thereof

By preparing the Mn(Ⅱ)-based metal halide material C46H52Br4MnP2, the high cost and high-temperature processing problems of existing X-ray scintillator materials have been solved, and a low-toxicity and efficient X-ray scintillator material with high spatial resolution and good performance has been achieved. Excellent radiation stability, suitable for medical diagnosis and industrial detection.

CN118724952AInactive Publication Date: 2024-10-01FUZHOU UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410730142.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing X-ray scintillator materials have high growth temperatures, difficult processing, high cost, and lack of low-toxicity and efficient luminescent materials, making it difficult to achieve high spatial resolution X-ray imaging.

Method used

The Mn(Ⅱ)-based metal halide material C46H52Br4MnP2 is prepared through the reaction of isopentyltriphenylphosphine and manganese bromide in an appropriate solvent to form (i-AmTPP)2MnBr4 crystal, and the scintillator screen is prepared by heating and melting. , achieving high transmittance and stability.

Benefits of technology

A low-cost, low-toxicity, easy-to-operate Mn(II)-based metal halide scintillator material with high spatial resolution and good radiation stability has been realized. The detection limit is as low as 45.71nGy s-1, and the radioluminescence intensity remains at 95.9 %, the spatial resolution reaches 52.5lp mm-1.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004879975870000011
    Figure FDA0004879975870000011
  • Figure HDA0004879976050000011
    Figure HDA0004879976050000011
  • Figure HDA0004879976050000012
    Figure HDA0004879976050000012
Patent Text Reader

Abstract

The invention discloses a Mn (II)-based metal halide scintillator material and a preparation method and application thereof, and belongs to the technical field of luminescent materials. The metal halide material has good response performance under excitation of blue light, ultraviolet light and X rays, the whole preparation process is simple and direct, conditions are mild, high-toxicity and high-pollution organic reagents and the like are not involved, and the used raw materials are low in price, low in cost and environmentally friendly. The Mn (II)-based metal halide material provided by the invention has good scintillation performance and radiation stability, and can realize X-ray imaging with high spatial resolution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of luminescent materials, and in particular relates to a Mn(II)-based metal halide scintillator material and a preparation method and application thereof. Background Art

[0002] With the development of science and technology, X-ray imaging detection technology has been widely used in medical imaging, industrial inspection, aerospace, and security fields. X-ray scintillators, as a type of material that can convert high-energy X-rays into low-energy ultraviolet or visible light, play a vital role in this. However, most of the commercialized scintillator materials are inorganic scintillator single crystals, which have problems such as high growth temperature, difficult processing, and high cost. In comparison, metal halide scintillators have many advantages, including low cost, simple preparation, and stable luminescence. Its unique photophysical and chemical properties, especially the structural regulation of the organic ligand part, can optimize its luminescence and stability properties. This makes metal halide materials one of the most anticipated candidate materials in the future development of scintillator materials.

[0003] After the X-ray scintillator material is irradiated, the excitons transition from the ground state to the high-energy excited state, and then undergo radiative transition to achieve X-ray excitation luminescence. Among them, low toxicity is the advantage of Mn (II)-based metal halides. The luminescence principle of Mn (II)-based metal halides is due to the fact that Mn 2+ dd transition, Mn 2+ The distance between metal centers will greatly affect its luminescence efficiency. By regulating the structure of organic ligands, the distance between metal centers can be regulated to improve the luminescence efficiency of the material. At the same time, its crystallinity can be regulated to obtain luminescent materials with better performance. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a Mn(II)-based metal halide luminescent material to achieve high spatial resolution X-ray imaging.

[0005] To achieve the above object, the present invention adopts the following technical solution:

[0006] In the first aspect, the present invention provides a Mn(II)-based metal halide material, whose chemical formula is C 46 H 52 Br4MnP 2, Abbreviated as (i-AmTPP)2MnBr4, where i-AmTPP + represents isopentyltriphenylphosphino.

[0007] In a second aspect, the present invention provides a method for preparing a Mn(II)-based metal halide crystal material, comprising the following steps:

[0008] (1) Dissolving isopentyltriphenylphosphonium bromide and manganese bromide in a certain proportion in an appropriate amount of solvent (selected from one, two or more of dichloromethane, ethanol, methanol, and N,N-dimethylformamide, preferably ethanol or a mixture of dichloromethane and ethanol) to form a saturated precursor solution.

[0009] (2) Adding or vapor-diffusion of solvent 2 into the solution in step (1) until light green crystals appear. Solvent 2 is selected from one or two of n-hexane, diethyl ether, and ethyl acetate, preferably diethyl ether.

[0010] In a third aspect, the present invention provides a scintillator screen comprising the above-mentioned Mn(II)-based metal halide scintillator.

[0011] In a fourth aspect, the present invention provides a heating and melting method for conveniently and quickly preparing the above-mentioned scintillator screen, which mainly comprises the following steps:

[0012] (1) The scintillator is placed on a glass sheet and heated to melt, and then placed in a vacuum oven to remove bubbles. Another glass sheet is placed on the molten liquid, and finally cooled back to room temperature to obtain the scintillator screen.

[0013] (2) The above-mentioned scintillator screen has extremely high optical transmittance.

[0014] In a fifth aspect, the present invention provides the use of the above-mentioned low-dimensional Mn(II)-based metal halide scintillator in the preparation of X-ray scintillator materials, such as a scintillator screen.

[0015] In a sixth aspect, the present invention provides the above-mentioned low-dimensional Mn(II)-based metal halide scintillator, and the application of the above-mentioned scintillator screen in the field of X-ray imaging, such as medical image detection or industrial detection.

[0016] The crystals prepared by the present invention are detected by a CCD single crystal X-ray diffractometer and are consistent with the structure of the target molecule, and the crystal quality is good and the yield is high.

[0017] The beneficial effects of the present invention are:

[0018] (1) The MnBr2 used in the present invention is cheap and low in toxicity, abundant on earth, and has a low cost for synthesis. The process of preparing the scintillator screen is simple, does not involve high temperature and high pressure, and is energy-saving and environmentally friendly.

[0019] (2) The (i-AmTPP)2MnBr4 of the present invention has good scintillation performance, and the light yield can reach 59101photons MeV -1 , detection limit as low as 45.71nGy s -1 , is the minimum dose rate of X-rays required for medical diagnosis (5.5 μGy s -1) is 1 / 108 of that of the conventional X-ray radiation. In addition, the present invention also evaluates its stability to X-ray radiation. -1 Under X-ray irradiation, the device was switched on and off 60 times in a cycle, and the radiation luminescence intensity remained at 95.9% of the original value, showing good radiation stability.

[0020] (3) The present invention can achieve high-resolution X-ray imaging, and the prepared scintillator screen can reach 52.5lp mm -1 The spatial resolution is much higher than that of most scintillator materials on the market, such as the 10lp mm of commercial inorganic scintillators (CsI:Tl). -1 . BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the crystal structure diagram of the metal halide material (i-AmTPP)2MnBr4.

[0022] Figure 2 Crystal powder diffraction XRD pattern and simulated XRD diffraction pattern of the metal halide material (i-AmTPP)2MnBr4.

[0023] Figure 3 Comparison diagram of photoluminescence PL and radioluminescence RL of metal halide material (i-AmTPP)2MnBr4.

[0024] Figure 4 The linear fitting curve of the luminescence intensity of the metal halide material (i-AmTPP)2MnBr4 under different X-ray radiation dose rates.

[0025] Figure 5 Figure 2 is the stability cycle diagram of the metal halide material (i-AmTPP)2MnBr4 after 40 minutes of X-ray irradiation.

[0026] Figure 6 X-ray imaging of the metal halide scintillator screen of (i-AmTPP)2MnBr4.

[0027] Figure 7 Modulation transfer function of metal halide scintillator screen imaging of (i-AmTPP)2MnBr4.

[0028] The (i-AmTPP)2MnBr4 in the present invention is C 46 H 52 Br4MnP 2。 DETAILED DESCRIPTION

[0029] In order to make the contents of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.

[0030] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0031] Example 1 Synthesis of (i-AmTPP)2MnBr4 Crystals

[0032] Dissolve isopentyltriphenylphosphonium bromide and MnBr2 in a small reagent bottle containing ethanol and dichloromethane solvent in a ratio of 2:1 to form a saturated precursor solution. Place the small reagent bottle into a large reagent bottle containing ether and let it stand for one day to obtain light green block crystals with the following crystal structure: Figure 1 shown.

[0033] Example 2 Preparation of (i-AmTPP)2MnBr4 Scintillator Screen

[0034] The (i-AmTPP)2MnBr4 single crystal or a mixture of isopentyltriphenylphosphonium bromide and MnBr2 in a certain proportion in Example 1 is placed on a glass slide and heated to melt, placed in a vacuum oven to remove bubbles, and covered with another glass slide on the molten liquid. Finally, it is cooled back to room temperature to obtain a high-transmittance (i-AmTPP)2MnBr4 scintillator screen.

[0035] Example 3 Experimental Analysis

[0036] The single crystal in Example 1 was collected by a RigakuAFC11 equipped with a Rigaku Saturn CCD area detector (Bruker-SMART), and the X-ray source was Mo-Kα ray

[0037] Powder X-ray diffraction (PXRD) patterns were obtained by Rigaku MiniFlex-II X-ray diffractometer using Cu-Kα radiation. get.

[0038] The photoluminescence spectrum of the crystal was measured at room temperature using a FLS980 fluorescence spectrometer, and the corresponding radioluminescence spectrum was measured by a FS5 fluorescence spectrometer.

[0039] The stability cycle diagram obtained under X-ray dose radiation for 40 minutes and the radioluminescence linear response diagram under different X-ray dose rates were measured by FS5 fluorescence spectrometer.

[0040] The X-ray imaging image is obtained by connecting an inverted fluorescence microscope to a portable X-ray tube, with the real object as the imaging object.

[0041] The modulation transfer function (MTF) is the transfer capability of the spatial frequency modulated by the input signal, and is generally used as an evaluation index of the spatial resolution performance of the imaging system. The present invention uses the bevel edge method to calculate the MTF curve. An X-ray image is taken using a tungsten sheet with a sharp edge, and the edge spread function (ESF) can be obtained from the inclined edge profile of the X-ray image. The MTF can be calculated by the following formula:

[0042] MTF(v)=F[LSF(x)]=F((dESF(x)) / dx)

[0043] Where v is the spatial frequency, x is the position of the pixel, the line spread function (LSF) is the derivative of the ESF, and the MTF is the Fourier transform of the LSF. The MTF of the image is then calculated using the software ImageJ.

[0044] Figure 2 This is the crystal powder XRD pattern of the metal halide material (i-AmTPP)2MnBr4. The peak position of the diffraction peak obtained by fitting the single crystal data is consistent with the peak position obtained by the powder X-ray diffraction test, indicating that it is a pure phase.

[0045] Figure 3 The comparison chart of the photoluminescence spectrum PL and the X-ray radiation luminescence spectrum RL of the metal halide crystal of (i-AmTPP)2MnBr4 shows that the emission sources of its radiation luminescence and photoluminescence are consistent.

[0046] Figure 4 The luminescence intensity fitting curve of the metal halide (i-AmTPP)2MnBr4 at different X-ray dose rates is shown in Figure 2. The detection limit of (i-AmTPP)2MnBr4 can be obtained by analysis. When the signal-to-noise ratio is 3, the luminescence intensity of (i-AmTPP)2MnBr4 corresponds to an X-ray dose rate of 45.71nGy s -1 , so its detection limit is 45.71nGy s -1 .

[0047] Figure 5 This is the stability cycle diagram of (i-AmTPP)2MnBr4 under 40min X-ray dose rate irradiation, indicating that it has good radiation stability.

[0048] Figure 6 This is the X-ray imaging of dried fish using the (i-AmTPP)2MnBr4 scintillator screen, indicating that the scintillator screen has good X-ray imaging capabilities.

[0049] Figure 7is the modulation transfer function of (i-AmTPP)2MnBr4 scintillator screen X-ray scintillator screen imaging. Through calculation, the modulation transfer function can accurately obtain the specific value of the material X-ray imaging spatial resolution. Figure 7 It can be seen that when the MTF value is equal to 0.2, the resolution of the (i-AmTPP)2MnBr4 scintillation screen is 52.5lp mm -1 .

[0050] Note: The chemical formula of (i-AmTPP)2MnBr4 is C 46 H 52 Br4MnP2.

[0051] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made according to the scope of the patent application of the present invention should fall within the scope of the present invention.

Claims

1. A Mn(II)-based metal halide scintillator material (i-AmTPP) 2MnBr4, characterized in that: The chemical formula is C 46 H 52 Br4MnP2, structural formula is as formula Ⅰ:

2. A method for preparing the Mn(II)-based metal halide scintillator material (i-AmTPP) 2MnBr4 as claimed in claim 1, characterized in that: Isoamyltriphenylphosphonium bromide and manganese bromide are dissolved in solvent 1 to form a saturated precursor solution, and solvent 2 is added by dropwise addition or vapor diffusion to prepare a Mn(II)-based metal halide scintillator crystal material (i-AmTPP)2MnBr4.

3. The method according to claim 2, characterized in that: The solvent 1 is at least one of dichloromethane, ethanol, methanol and N,N-dimethylformamide; the solvent 2 is at least one of n-hexane, ether and ethyl acetate.

4. A method for preparing the Mn(II)-based metal halide scintillator material (i-AmTPP) 2MnBr4 as claimed in claim 1, characterized in that: Isoamyltriphenylphosphonium bromide and manganese bromide are mixed and fully ground, heated to melt, and cooled and solidified to obtain a Mn(Ⅱ)-based metal halide scintillator glass material (i-AmTPP) 2MnBr4.

5. A method for preparing the Mn(II)-based metal halide scintillator material (i-AmTPP) 2MnBr4 as claimed in claim 1, characterized in that: Isoamyltriphenylphosphonium bromide and manganese bromide are dissolved in solvent 1 to form a saturated precursor solution, and solvent 2 is added by dropwise addition or vapor diffusion to obtain a Mn(Ⅱ)-based metal halide scintillator crystal material (i-AmTPP)2MnBr4, which is heated to melt and cooled and solidified to obtain a Mn(Ⅱ)-based metal halide scintillator glassy material (i-AmTPP)2MnBr4.

6. The method according to any one of claims 2, 4 and 5, characterized in that: The molar ratio of isopentyltriphenylphosphonium bromide to manganese bromide is 2:

1.

7. An application of the Mn(II)-based metal halide scintillator material (i-AmTPP) 2MnBr4 as claimed in claim 1, characterized in that: The scintillator material is used to prepare X-ray imaging and detection materials.

8. The use according to claim 7, characterized in that: The scintillator material is used to prepare a scintillator screen.

9. The use according to claim 7, characterized in that: The preparation method of the scintillating screen is as follows: placing the Mn(Ⅱ)-based metal halide scintillator material (i-AmTPP)2MnBr4 on glass and heating it to melt, and after no bubbles appear in the melt, taking another glass sheet to cover the melt, then slowly cooling it down, removing the surface glass sheet, and obtaining the scintillating screen.

10. An application of the Mn(II)-based metal halide scintillator material (i-AmTPP) 2MnBr4 as claimed in claim 1, characterized in that: The scintillator material is used to prepare the light-emitting layer material of a doped or non-doped OLED device.

Citation Information

Patent Citations

  • Low-dimensional Mn (II)-based organic-inorganic metal halide scintillator with high spatial resolution