Slurry composition, soft polishing pad and preparation method thereof

By using a slurry composition of polyurethane, anionic additives and nonionic additives in the soft polishing pad to form a through-hole structure, the problems of insufficient polishing efficiency and wear resistance of the existing soft polishing pads are solved, and the problem is achieved Efficient and low-cost polishing processing.

CN118725709APending Publication Date: 2024-10-01HUBEI DINGLONG HUISHENG MATERIALS CO LTD +2
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202311853503.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing soft polishing pads have deficiencies in polishing efficiency and wear resistance, and low mechanical strength, resulting in low processing efficiency and high cost.

Method used

A slurry composition is used, including polyurethane, anionic additives and nonionic additives, and is cross-linked and solidified to form finger-like and sponge-like through-hole structures to improve the transportation efficiency and mechanical strength of the polishing fluid, and prepare a polishing liquid with Soft polishing pad with high polishing efficiency and wear resistance.

Benefits of technology

It improves polishing efficiency and wear resistance, reduces processing costs, and achieves a more efficient polishing process and better mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725709A_ABST
    Figure CN118725709A_ABST
Patent Text Reader

Abstract

The invention provides a slurry composition, a soft polishing pad and a preparation method of the soft polishing pad, and relates to the field of chemical mechanical polishing. The slurry composition provided by the invention is prepared from the following components in parts by mass: 100 parts of polyurethane, 1 to 4 parts of an anionic auxiliary agent and 1 to 4 parts of a nonionic auxiliary agent, and the number-average molecular weight of the nonionic auxiliary agent is 15000 to 25000. The soft polishing pad prepared from the slurry composition is high in polishing efficiency and good in wear resistance, the processing efficiency of wafers is improved, and the processing cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of chemical mechanical polishing, and in particular to a slurry composition, a soft polishing pad and a preparation method thereof. Background Art

[0002] Chemical Mechanical Polishing (CMP) is a process technology that can achieve global planarization. It is widely used in ultra-precision surface processing fields such as integrated circuits, computer heads, and hard disks. CMP technology can achieve nano-level surface accuracy and sub-nanometer surface roughness processing, while the surface and sub-surface are not damaged. The basic principle of CMP technology is: the wafer to be polished is pressed between the elastic polishing pad and the polishing head, and then the wafer and the polishing pad rotate in the same direction, and then a continuously flowing polishing slurry is added between the wafer and the polishing pad. Under high-speed operation, the reaction products on the surface of the polished wafer are continuously peeled off, and new polishing slurry is replenished, and the reaction products are taken away with the polishing slurry. The newly exposed wafer plane undergoes chemical reactions again, and the products are peeled off again and the cycle repeats. Under the combined action of the substrate, abrasive particles and chemical reagents, an ultra-precision surface is formed. In this process, the polishing pad mainly plays the role of storing and transporting polishing liquid, removing abrasive debris and maintaining a stable polishing environment.

[0003] In the prior art, polishing pads are mainly divided into two types: hard polishing pads and soft polishing pads according to different materials. Among them, soft polishing pads are generally made of thermoplastic polyurethane, which has a good flattening effect and can also achieve a low defect rate; however, soft polishing pads have low mechanical strength and poor wear resistance, and the polishing efficiency is not high in actual use. Summary of the invention

[0004] The embodiments of the present application can provide a slurry composition, a soft polishing pad and a preparation method thereof. The slurry composition can prepare a soft polishing pad with high polishing efficiency and good wear resistance, which is beneficial to improving the processing efficiency of wafers and reducing processing costs.

[0005] In a first aspect, an embodiment of the present application provides a slurry composition, whose components, measured in parts by mass, include 100 parts of polyurethane, 1 to 4 parts of anionic additives, and 1 to 4 parts of non-ionic additives, and the number average molecular weight of the non-ionic additive is 15,000 to 25,000.

[0006] In the above technical scheme, the slurry composition will be mixed with a good solvent when it is used. At this time, polyurethane, as the matrix resin of the slurry composition, can be cross-linked and cured in a liquid environment, thereby promoting the overall curing of the slurry composition. With polyurethane as the matrix resin, the slurry composition has good mechanical strength and wear resistance after curing. The anionic additives and non-ionic additives in the slurry composition act synergistically during the cross-linking and curing process of the polyurethane, and can promote the formation of two different types of pore structures, namely, finger-shaped through holes and sponge-shaped through holes, which are interconnected, so that the cured slurry composition has the function of storing and transporting polishing liquid. Among them, the finger-shaped channel has a longer length and a larger inner diameter, and the sponge-shaped through hole has a smaller size. The finger-shaped channel and the sponge-shaped through hole are used in combination to store the polishing liquid and transport the polishing liquid to the surface.

[0007] The inventors found that appropriately increasing the aperture of the sponge-like through-holes is beneficial to improving the transportation efficiency of the polishing liquid; the non-ionic additive with a number average molecular weight of 15,000 to 25,000 can make the poor solvents gather together better when the slurry composition is solidified, thereby appropriately increasing the aperture of the sponge-like through-holes, which is beneficial to improving the transportation efficiency of the solidified slurry composition for the polishing liquid. The anionic additive can increase the exchange rate between the slurry composition and the external poor solvent when the slurry composition is solidified, which is beneficial to the formation of finger-shaped through-holes. Therefore, when the slurry composition is used to prepare a soft polishing pad, the synergistic effect of the anionic additive and the non-ionic additive can improve the polishing efficiency of the solidified slurry composition. In addition, the amount of the non-ionic additive and the anionic additive in the slurry composition also needs to be controlled within a suitable range. If the amount of the non-ionic additive is too small, it is not easy to form a sponge through-hole with a larger aperture, which is not conducive to improving the grinding efficiency; if the amount of the non-ionic additive is too much, it will play a lubricating role in the polishing process, reduce the friction coefficient, and reduce the grinding efficiency. If the amount of the anionic auxiliary agent used is too much, the wear resistance of the formed soft polishing pad will be deteriorated.

[0008] In a possible implementation, the nonionic auxiliary agent includes at least one of a polyol type, a polyoxyethylene type, and a polyether-modified silicone; optionally, the nonionic auxiliary agent is a polyether-modified silicone.

[0009] In the above technical solution, the inventors found that when polyether-modified silicone is used as a non-ionic auxiliary agent in the slurry composition, it can better improve the polishing efficiency of the slurry composition after curing.

[0010] In one possible implementation, the polyurethane includes at least one of polyester polyurethane, polyether polyurethane, and polycarbonate polyurethane; and / or the anionic auxiliary agent includes at least one of higher fatty acid ester salts, sulfonated salts, sulfate ester salts, and phosphate ester salts.

[0011] In one possible implementation, the components of the slurry composition also include an organic solvent, and the solid content of the slurry composition is 18% to 22% based on the polyurethane; optionally, the organic solvent includes at least one of N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), methyl ethyl ketone (2-Butanone, MEK), cyclohexanone (CHN), tetrahydrofuran (THF), and 1,4-dioxane.

[0012] In the above technical scheme, the organic solvent acts as a good solvent, which can dissolve and evenly disperse other components such as polyurethane in the slurry composition, and can provide a liquid environment for curing of the slurry composition, and can also ensure the uniformity of the slurry composition; and the solid content in the range of 18% to 22% is beneficial to ensure the appropriate viscosity of the slurry composition, and is beneficial to the curing and film formation of the slurry composition.

[0013] In a possible implementation, the slurry composition further includes 2 to 4 parts by mass of a filler; optionally, the filler includes at least one of carbon black, polyvinyl chloride and its derivatives, cellulose and its derivatives, and polymer microspheres.

[0014] In the above technical solution, the filler can play a reinforcing role, so that the slurry composition has better mechanical strength after curing.

[0015] In a second aspect, an embodiment of the present application provides a soft polishing pad, which includes a polishing layer and a base film layer, the polishing layer and the base film layer are stacked, and the polishing layer is formed by curing the above-mentioned slurry composition.

[0016] In the above technical solution, the base film layer plays the role of supporting the polishing layer, and the polishing layer can play the role of storing and transporting the polishing liquid. The polishing layer formed by curing the above slurry composition has higher polishing efficiency, stronger mechanical strength and better wear resistance.

[0017] In the third aspect, the soft polishing pad provided in the embodiment of the present application includes a polishing layer and a base film layer which are stacked together, and a number of finger-shaped channels are evenly distributed in the polishing layer. An opening is provided at one end of each finger-shaped channel, and the opening is located on the surface of the polishing layer away from the base film layer, and the other end of the finger-shaped channel extends toward the base film layer along the thickness direction of the polishing layer; sponge holes are provided between at least some of the finger-shaped channels, and the sponge holes are connected to the finger-shaped channels adjacent to them; the average inner diameter of the finger-shaped channels is 35μm to 65μm, and the average pore diameter of the sponge holes is 5μm to 15μm.

[0018] In the above technical solution, the base film layer of the soft polishing pad can play the role of bearing the polishing layer, and the polishing layer can play the role of storing and transporting the polishing liquid. When the soft polishing pad is used, the polishing liquid can be transported to the surface of the polishing layer through the opening of the finger-shaped channel, and then the wafer to be processed is polished; the sponge through holes with an average pore size of 5μm to 15μm between the finger-shaped channels can not only play the role of storing the polishing liquid, but also ensure the connection between adjacent finger-shaped channels, which is conducive to increasing the transportation efficiency of the polishing liquid, thereby improving the polishing efficiency.

[0019] In a possible implementation, the material of the base film layer is any one of polyethylene terephthalate (PET), polypropylene (PP), and polyethylene (PE).

[0020] In a fourth aspect, an embodiment of the present application provides a method for preparing a soft polishing pad, which comprises the following steps: applying the above-mentioned slurry composition to the surface of a base film, and then immersing the slurry composition in a coagulation liquid until the slurry composition is solidified.

[0021] In the above technical solution, the soft polishing pad prepared by using the above slurry composition has high polishing efficiency and good wear resistance.

[0022] In a possible implementation, the main component of the coagulation liquid includes at least one of water, ethanol, methanol, and isopropanol.

[0023] In the above technical solution, water, ethanol, methanol and isopropanol have poor solubility in polyurethane and can promote rapid solidification of the slurry composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments of the present application will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is a SEM image of the soft polishing pad formed by curing in Example 1 of the present application;

[0026] Figure 2 This is a SEM image of the soft polishing pad formed by curing in Example 2 of the present application;

[0027] Figure 3 This is a SEM image of the soft polishing pad formed by curing in Example 3 of the present application.

[0028] Figure 4 This is a SEM image of the soft polishing pad formed by curing in Example 4 of the present application. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0030] The slurry composition, the soft polishing pad and the preparation method thereof according to the embodiments of the present application are described in detail below.

[0031] In the embodiment of the present application, the slurry composition contains a solute and an organic solvent, wherein the components of the solute, measured by weight, contain 100 parts of polyurethane, 1 to 4 parts of anionic additives, 1 to 4 parts of non-ionic additives, and 2 to 4 parts of fillers, wherein the number average molecular weight of the non-ionic additive is 15,000 to 25,000; and based on the amount of polyurethane, the solid content of the slurry composition is generally 18% to 22%.

[0032] In the embodiment of the present application, the organic solvent plays a role in dissolving and uniformly dispersing the solute to ensure the uniformity of the slurry composition. Specifically, the organic solvent in the embodiment of the present application generally includes at least one of N,N-dimethylformamide, dimethyl sulfoxide, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and 1,4-dioxane; as an example, the organic solvent in this embodiment uses N,N-dimethylformamide.

[0033] Polyurethane is used as the base resin in the slurry composition, and can crosslink and cure with each other, so that the slurry composition is cured. The slurry composition with polyurethane as the base resin has good mechanical strength and wear resistance after curing. The polyurethane in the embodiment of the present application includes at least one of polyester polyurethane, polyether polyurethane, and polycarbonate polyurethane, among which the slurry composition with polyester polyurethane as the base resin has the best wear resistance after curing.

[0034] Polyurethane can be purchased on the market or obtained by self-production. The functions of the two are the same. They are used as the base resin of the slurry composition to ensure that the slurry composition can solidify when used. Taking polyester polyurethane as an example, the first polymer is prepared when it is made by itself: polyester polyol reacts with isocyanate to generate a hydroxyl-terminated prepolymer, and the second polymer is prepared: a chain extender, isocyanate and a diluent are added to the first polymer to obtain a polyester polyurethane with an expected molecular weight. If it is a polyester-polyether composite resin, the first polymer is prepared by: polyester polyol and polyether polyol react with isocyanate to generate a hydroxyl-terminated prepolymer; the second polymer is prepared by: adding a chain extender, isocyanate and a diluent to the first polymer to obtain a polyester-polyether composite resin with an expected molecular weight. Moreover, after the polymerization is completed, methanol will be added to quench the activity of raw materials such as isocyanate to ensure that there are almost no active groups in the polyurethane. In order to ensure that the molecular weight of the polymer is accurately controlled and concentrated, the polyurethanes used in the embodiments of this application are all homemade.

[0035] Anionic additives and nonionic additives can promote the formation of channels and pore-like structures during the curing process of the slurry composition. Among them, the anionic additive can increase the exchange rate between the organic solvent (i.e., DMF) in the slurry composition and the poor solvent (i.e., water) in the coagulation liquid when the slurry composition is cured, which is conducive to the formation of finger-shaped channels (referred to as finger-shaped channels), which can transport the polishing liquid to the surface of the cured film. At this time, the amount of anionic additives should be controlled within a suitable range. If the amount is too much, it is easy to cause the wear resistance of the formed soft polishing pad to deteriorate; if the amount is too little, it is not easy to form a finger-shaped channel of suitable size; in the embodiment of the present application, the anionic additive includes at least one of higher fatty acid ester salts (such as higher fatty acid sodium, etc.), sulfonated salts (such as sodium diisooctyl sulfosuccinate, etc.), sulfate ester salts (such as sodium lauryl sulfate, etc.), and phosphate ester salts (such as potassium hexadecyl phosphate, etc.). When the slurry composition is cured, the non-ionic additive can promote the formation of sponge-like through holes (referred to as sponge through holes) between the finger-shaped channels that are connected to the slurry composition. The sponge through holes can not only store the polishing liquid, but also ensure the connection between adjacent finger-shaped channels; and the inventors have found that appropriately increasing the pore size of the sponge-like through holes is conducive to improving the transportation efficiency of the polishing liquid. In addition, the inventors have also found that when the number average molecular weight of the non-ionic additive is 15,000 to 25,000, the poor solvent will be more likely to gather together when the slurry composition is cured, which is more conducive to appropriately expanding the pore size of the sponge through holes, thereby improving the transportation efficiency of the polishing liquid. In the embodiment of the present application, the non-ionic additive generally includes at least one of a polyol type, a polyoxyethylene type, and a polyether-modified silicone. The polyol type includes anhydrous sorbitan monooleate, etc., and the polyoxyethylene type includes fatty alcohol polyoxyethylene ether, etc. Among them, the non-ionic additives such as polyether-modified silicone are particularly effective in improving the pore size of the sponge through holes. Polyether-modified silicone is formed by graft copolymerization of polyether and dimethylsiloxane, which can be obtained from the market or made by yourself. When making it yourself, the polyether includes but is not limited to at least one of polyethylene glycol and polypropylene glycol, and polyethylene glycol (PEG600) is generally selected; dimethylsiloxane is preferably dimethylsiloxane is polydimethylsiloxane (PDMS1000); the preferred ratio between the polyether segment and the polydimethylsiloxane segment is 1:2. In the embodiment of the present application, the polyether-modified silicone is commercially available. In addition, it should be noted that the mass fraction of non-ionic additives with a number average molecular weight of 15000 to 25000 needs to be controlled within an appropriate range. If the amount of non-ionic additives is too small, it is not easy to form sponge pores with larger pores, which is not conducive to improving the grinding efficiency; if the amount of non-ionic additives is too much, it will play a lubricating role in the polishing process, reduce the friction coefficient, and reduce the grinding efficiency instead.

[0036] The nonionic additives and anionic additives in the embodiments of the present application work synergistically to form sponge pores and finger-type channels that are interconnected when the slurry composition is cured. In this way, the soft polishing pad prepared using the slurry composition can play the role of storing and transporting the polishing liquid. Moreover, since the nonionic additives with a number average molecular weight of 15,000 to 25,000 can appropriately increase the pore size of the sponge pores, the slurry composition has better polishing liquid transmission capabilities after curing, thereby improving the polishing efficiency of the soft polishing pad.

[0037] The filler can improve the strength of the slurry composition, so that the cured slurry composition has better mechanical strength, and in some other embodiments, the filler can also be selected according to the situation. The filler includes at least one of carbon black, polyvinyl chloride and its derivatives, cellulose and its derivatives, and polymer microspheres.

[0038] The embodiment of the present application also provides a soft polishing pad, which includes a polishing layer and a base film layer, the polishing layer and the base film layer are stacked, and the polishing layer is formed by curing the above-mentioned slurry composition.

[0039] In addition, in the soft polishing pad of the embodiment of the present application, finger-shaped channels and sponge holes are provided in the polishing layer, and a plurality of finger-shaped channels are distributed. An opening is provided at one end of each finger-shaped channel, and the opening is located on the surface of the polishing layer away from the base film layer, and the other end of the finger-shaped channel extends toward the base film layer along the thickness direction of the polishing layer; sponge holes are provided between at least some of the finger-shaped channels, and the sponge holes are connected to the finger-shaped channels adjacent thereto; the average inner diameter of the finger-shaped channels is 35μm to 65μm, and the average pore diameter of the sponge holes is 5μm to 15μm.

[0040] In the soft polishing pad in the embodiment of the present application, the base film layer plays the role of supporting the polishing layer, and the material of the base film layer can be selected from any one of polyethylene terephthalate, polypropylene, and polyethylene; specifically in the embodiment and application example of the present application, the material of the base film layer is polyethylene terephthalate. The polishing layer plays the role of storing and transporting the polishing liquid; when the soft polishing pad is used for CMP polishing, the polishing liquid will be transported to the surface of the polishing layer through the finger-shaped channels and sponge through holes in the polishing layer to polish the wafer to be processed. Compared with the existing soft polishing pad, the soft polishing pad in the embodiment of the present application has a good ability to transport the polishing liquid because the average pore size of the sponge through hole is 5μm to 15μm, and thus has excellent polishing efficiency. In addition, since the base resin in the polishing layer in the embodiment of the present application is polyurethane, it also has good mechanical properties and wear resistance.

[0041] The present application also provides a method for preparing a soft polishing pad, which comprises the following steps:

[0042] S100, curing: coating a slurry composition containing an organic solvent on the surface of the base film layer, and then immersing the slurry composition in a coagulation liquid until the slurry composition is cured to form a polishing layer.

[0043] The operation of wet film formation by introducing the polymer solution into the coagulation liquid is generally referred to as the "phase inversion method". In the phase inversion method, the main component of the coagulation liquid is generally a poor solvent, such as at least one of water, ethanol, methanol, and isopropanol; the secondary component is a good solvent, which can be the same as the organic solvent in the slurry composition. As an example, in the subsequent embodiments and application examples of this application, the coagulation liquid is a 10% DMF aqueous solution, and the organic solvent is DMF.

[0044] In this step, the curing principle of the slurry composition is as follows:

[0045] The components such as polyurethane in the slurry composition are evenly dispersed in DMF, so the slurry composition has good uniformity at the beginning. As the slurry composition enters the coagulation liquid, water phase separation will occur inside the slurry composition to form finger-shaped channels; at the same time, the diffusion of water molecules causes a lot of scattered water molecules to exist inside the liquid slurry composition, and these water molecules will aggregate with each other. When they aggregate to a certain amount, the DMF in the slurry composition is not enough to dissolve the polyurethane, so the polyurethanes will cross-link and solidify to form sponge through holes connected to the finger-shaped channels in the aggregated water molecule area.

[0046] In this step, the anionic additive in the slurry composition can increase the exchange rate, thereby promoting the rapid formation of finger-type channels; the hydrophilic effect of the non-ionic additive with a number average molecular weight of 15,000 to 25,000 can make the number of water molecules reach a larger scale, thereby appropriately increasing the pore size of the sponge through-holes; taking the polyether modifier silicone as an example, the hydrophilic end of the polyether modifier silicone can effectively aggregate free water molecules, while the hydrophobic end slows down the exchange of water molecules with DMF, so that the free water molecules have a longer aggregation time, thereby forming larger water molecule clusters. Therefore, under the synergistic effect of the anionic additive and the non-ionic additive, the polishing layer has a good ability to transport the polishing liquid; and because the base resin of the polishing layer is polyurethane, the polishing layer formed by curing also has good mechanical strength and wear resistance.

[0047] S200, post-processing: drying, grinding, embossing and other processing processes are performed on the polishing layer and the base film layer.

[0048] After the polishing layer is solidified, the polishing layer and the base film layer need to be further processed to obtain a soft polishing pad suitable for industrial production requirements. Since the drying, grinding, embossing and other processing processes are relatively conventional and are not the focus of this application, this application will not repeat the detailed process here, and the specific process can be referred to the prior art.

[0049] The features and performance of the present application are further described in detail below in conjunction with the embodiments.

[0050] Synthesis example 1

[0051] Synthesis of Polyester Polyurethane

[0052] 1) Preparation of the first polymer: heat the polyester diol to 140°C, evacuate to -0.1MPa, until no liquid is discharged, and measure the water content to be <150ppm; add it into a reaction kettle, mix it evenly, then add isocyanate to react, control the isocyanate index R=0.80, the reaction temperature is 85°C, seal the reaction at normal pressure for 3h, then add DMF to dilute.

[0053] 2) Preparation of the second polymer: Ethylene glycol, diphenylmethane diisocyanate (4,4'-diphenylmethanediisocyanate, MDI) and DMF were added to the first polymer, the total isocyanate index R was controlled to be 1.02, and the reaction was carried out at 85°C and normal pressure; the number average molecular weight was detected every 2 hours, and when the number average molecular weight reached the target value of 70,000, the end-capping agent methanol was added to terminate the reaction.

[0054] Synthesis example 2

[0055] 1) Synthesis of polyester-polyether composite resin

[0056] Preparation of the first polymer: Mix the polyester diol and the polyether triol and heat them to 140°C, evacuate to -0.1MPa until no liquid is discharged, and measure the moisture content to be <150ppm; add them into the reactor, mix them evenly, then add isocyanate to react, control the isocyanate index R1=0.80, the reaction temperature is 85°C, seal the reaction at normal pressure for 3h, then add DMF to dilute.

[0057] (2) Preparation of the second polymer: Ethylene glycol, MDI and DMF were added to the first polymer, the total isocyanate index R was controlled to be 1.02, and the reaction was carried out at 85°C and normal pressure; the number average molecular weight was detected every 2 hours, and when the number average molecular weight reached the target value of 70,000, the end-capping agent methanol was added to terminate the reaction.

[0058] Example 1

[0059] This embodiment provides a slurry composition, and its components, calculated by weight, are as follows:

[0060] 100 parts of the polyester polyurethane of Synthesis Example 1, 2 parts of sodium diisooctyl sulfosuccinate, 2 parts of polyether-modified silicone with a number average molecular weight of 21789, 2.4 parts of carbon black, and the solid content of the polyester polyurethane is 30%, and the organic solvent is DMF.

[0061] Example 2

[0062] This embodiment provides a slurry composition, and the main difference between its components and those of Embodiment 1 is that 2 parts of sorbitan monooleate are used instead of polyether-modified silicone as a non-ionic auxiliary agent.

[0063] Example 3

[0064] This embodiment provides a slurry composition, and its components are mainly different from those of Example 1 in that 100 parts of the polyester-polyether composite resin of Synthesis Example 2 are used instead of the polyester polyurethane of Synthesis Example 1.

[0065] Example 4

[0066] This embodiment provides a slurry composition, and the main difference between its components and those of Embodiment 3 is that 2 parts of sorbitan monooleate are used instead of polyether-modified silicone as the non-ionic auxiliary agent.

[0067] Comparative Example 1

[0068] This comparative example provides a slurry composition, and its components are mainly different from those of Example 1 in that the number average molecular weight of the polyether-modified silicone is 29187.

[0069] Comparative Example 2

[0070] This comparative example provides a slurry composition, and the components thereof are mainly different from those of Example 1 in that the number average molecular weight of the polyether-modified silicone is 11462.

[0071] Comparative Example 3

[0072] This comparative example provides a slurry composition, and the main difference between the components of the slurry composition and those of Example 1 is that the slurry composition does not contain a polyether-modified silicone resin.

[0073] Comparative Example 4

[0074] This comparative example provides a slurry composition, and its components are mainly different from those of Example 1 in that the amount of sodium diisooctyl sulfosuccinate is 5 parts.

[0075] Comparative Example 5

[0076] This comparative example provides a slurry composition, and its components are mainly different from those of Example 1 in that the amount of polyether-modified silicone is 5 parts.

[0077] Comparative Example 6

[0078] This comparative example provides a slurry composition, and its components are mainly different from those of Example 1 in that the amount of polyether-modified silicone is 0.8 parts.

[0079] Application Examples

[0080] According to the preparation method of the soft polishing pad described above, the slurry compositions in Examples 1 to 4 and Comparative Examples 1 to 6 were used to prepare soft polishing pads, and each soft polishing pad was numbered according to the slurry composition, and its performance was tested.

[0081] The inventors also tried to use a slurry composition without anionic additives to prepare a soft polishing pad, but found that the slurry composition without anionic additives could not transport the polishing liquid after curing, so the present application did not conduct further testing on it.

[0082] Through-hole performance test

[0083] The SEM images of the polishing pad surface and the through holes at the cross section were taken using a scanning electron microscope (SEM), and the obtained SEM images were analyzed using Image Pro Plus 6.0 software to obtain the surface pore size (i.e., the pore size at the opening of the finger-shaped channel) and the sponge pore size. The detailed data are shown in Table 1. The present application provides SEM images of the soft polishing pad formed by curing the slurry composition of Examples 1 to 4, which correspond to Figure 1 to Figure 4 .

[0084] Figure 1 to Figure 4 In each figure, from left to right, there are SEM images of the cross section of the corresponding polishing pad, SEM images of the finger-shaped channels, and SEM images of the sponge through holes.

[0085] Wear resistance test

[0086] The polishing machine model UNI-POL-802 of Shenyang Kejing Automation Co., Ltd. was used for testing. Huida disk DK3601 was used, and the total load was 3.9kg, the rotation speed was 200rpm, the water flow rate was 1.15L / min, and the polishing time was 20min. Each soft polishing pad sample was tested. The consumption of the polishing pad groove was tested and recorded. The greater the consumption, the worse the wear resistance of the polishing pad.

[0087] Polishing efficiency test

[0088] The copper barrier layer on the silicon wafer was polished using the Dingze DB2801 polishing liquid and the Ebara 300X polishing machine of Japan Ebara Machinery to determine the polishing efficiency (RR) of each soft polishing pad. The polishing parameters are: head pressure of 2.5psi, polishing liquid flow rate of 300ml / min. The polishing data of the test wafer was recorded, and the RR of 5 consecutive wafers was counted and the average value was calculated as the recorded data. The results are shown in Table 1.

[0089] Table 1 Performance test results of embodiments and comparative examples

[0090]

[0091] From the above results, it can be found that the soft polishing pad made of the slurry composition of the embodiment of the present application has a good polishing efficiency compared with the comparative example. And as shown in Table 1, compared with Example 2 and Example 4, Example 1 and Example 3 using polyether-modified silicone as the non-ionic auxiliary agent of the slurry composition have larger sponge pores, indicating that the polyether-modified silicone has a particularly significant improvement in the transport rate of the soft polishing pad, thereby further improving the grinding efficiency of the soft polishing pad. And from the comparison of Example 1 and Example 3, and the comparison of Example 2 and Example 4, it can be seen that the wear resistance of the soft polishing pad is also significantly improved by using polyester polyurethane as the base resin.

[0092] The above are only embodiments of the present application and are not intended to limit the scope of protection of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the scope of protection of the present application.

Claims

1. A slurry composition, It is characterized in that The components thereof include 100 parts of polyurethane, 1 to 4 parts of anionic additives and 1 to 4 parts of nonionic additives by weight, and the number average molecular weight of the nonionic additives is 15000 to 25000.

2. The slurry composition according to claim 1, It is characterized in that The nonionic auxiliary agent includes at least one of a polyol type, a polyoxyethylene type, and a polyether-modified silicone; optionally, the nonionic auxiliary agent is a polyether-modified silicone.

3. The slurry composition according to claim 1, It is characterized in that The polyurethane comprises at least one of polyester polyurethane, polyether polyurethane and polycarbonate polyurethane; And / or, the anionic auxiliary agent includes at least one of higher fatty acid ester salts, sulfonated salts, sulfate ester salts, and phosphate ester salts.

4. The slurry composition according to claim 1, It is characterized in that Its components also include an organic solvent, and based on the polyurethane, the solid content of the slurry composition is 18% to 22%; optionally, the organic solvent includes at least one of N,N-dimethylformamide, dimethyl sulfoxide, methyl ethyl ketone, cyclohexanone, tetrahydrofuran, and 1,4-dioxane.

5. The slurry composition according to claim 1, It is characterized in that The components also include 2 to 4 parts by mass of filler; optionally, the filler includes at least one of carbon black, polyvinyl chloride and its derivatives, cellulose and its derivatives, and polymer microspheres.

6. A soft polishing pad, It is characterized in that The invention comprises a polishing layer and a base film layer, wherein the polishing layer and the base film layer are stacked and arranged, and the polishing layer is formed by curing the slurry composition according to any one of claims 1 to 5.

7. A soft polishing pad, It is characterized in that It comprises a polishing layer and a base film layer which are stacked together, wherein a plurality of finger-shaped channels are distributed in the polishing layer, wherein an opening is arranged at one end of each of the finger-shaped channels, wherein the opening is located on the surface of the polishing layer away from the base film layer, and the other end of the finger-shaped channel extends toward the base film layer along the thickness direction of the polishing layer; sponge through holes are arranged between at least some of the finger-shaped channels, and the sponge through holes are connected with the finger-shaped channels adjacent thereto; the average inner diameter of the finger-shaped channels is 35 μm to 65 μm, and the average pore diameter of the sponge through holes is 5 μm to 15 μm.

8. The soft polishing pad according to claim 6 or 7, It is characterized in that The material of the base film layer is any one of polyethylene terephthalate, polypropylene and polyethylene.

9. A method for preparing a soft polishing pad, It is characterized in that It includes the following steps: The slurry composition according to any one of claims 1 to 5 is applied to a surface of a base film, and then the slurry composition is immersed in a coagulation liquid until the slurry composition is solidified.

10. The method for preparing the soft polishing pad according to claim 9, It is characterized in that The main component of the coagulation liquid includes at least one of water, ethanol, methanol and isopropanol.

Citation Information

Cited By

  • Polishing pad and preparation method thereof

    CN121156908A

  • Polishing pad with double-layer hole structure as well as preparation method and application of polishing pad

    CN121670516A