Preparation method of ultra-coarse-grain tungsten-cobalt hard alloy

By adding reinforcing components and anti-wear toughening agents during the preparation process of tungsten-cobalt cemented carbide, the coupling structure of the tungsten carbide grain morphology and the alloy phase is improved, and the problem of poor performance of tungsten-cobalt cemented carbide in the existing technology is solved. problem and achieved the preparation of ultra-coarse-grained tungsten-cobalt cemented carbide with high hardness and toughness.

CN118726786AInactive Publication Date: 2024-10-01ZHUZHOU KIMBERLY CEMENTED CARBIDE CO LTD

Patent Information

Application Number
CN202410657217.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-25
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of tungsten-cobalt cemented carbide is prone to uneven metallographic structures, short light ball milling time, and low mixing strength, resulting in poor alloy performance and difficulty in preparing ultra-coarse-crystalline tungsten with high hardness and good toughness. Cobalt carbide.

Method used

Adopting a preparation method, including wet grinding ultra-coarse tungsten carbide and cobalt powder in a ball mill, adding reinforcing components and anti-wear toughening agents, sintering under vacuum conditions after granulation and pressing, and controlling the sintering temperature and heating rate. Modified niobium carbide and anti-wear toughening agent are used to improve the tungsten carbide grain morphology and the toughness of the alloy phase.

Benefits of technology

By improving the coupling structure of the tungsten carbide grain morphology and the alloy phase, the toughness and hardness of the alloy are improved, and the preparation of high-performance ultra-coarse-grained tungsten-cobalt cemented carbide is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004858312910000041
    Figure BDA0004858312910000041
  • Figure BDA0004858312910000101
    Figure BDA0004858312910000101
Patent Text Reader

Abstract

The invention discloses an ultra-coarse grain WC-Co hard alloy and a preparation method thereof, and belongs to the technical field of powder metallurgy, and the preparation method comprises the following steps: S1, preparing the following raw materials in parts by weight; step S2, preparation of a mixture; step S3, carrying out granulation treatment; step S4, pressing; step S5, sintering; according to the invention, the reinforcing component and the anti-wear toughening agent are added, niobium carbide in the reinforcing component can change the form of tungsten carbide grains, KH-550 coated on modified niobium carbide can be chemically bonded with hydroxyl groups on chitosan and polyvinyl alcohol, and meanwhile, a compound solution of chitosan and polyvinyl alcohol has excellent adhesion, so that the wear resistance of the lubricating oil is improved, and the service life of the lubricating oil is prolonged. The wear-resistant toughening agent can be mutually coupled with hard units of tungsten carbide and cobalt alloy, the wear-resistant toughening agent is prepared from an inorganic nano metal base material, a phosphoric acid solution and modified silica sol, and the toughness and hardness of the alloy are jointly improved through the combined action of all the structures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder metallurgy, in particular to a method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide. Background Art

[0002] Tungsten-cobalt cemented carbide is a metal material composed of refractory metal compound WC and bonding phase Co, which is prepared by adjusting the material formula, molding process, and high-temperature sintering under a protective atmosphere. Among them, the WC grain size is closely related to the performance of cemented carbide.

[0003] With the development of science and technology, people have put forward higher requirements on the performance of tungsten-cobalt cemented carbide. Ultra-coarse-grained cemented carbide has excellent wear resistance, thermal fatigue resistance and thermal shock resistance under extreme working conditions and continuous operation. It is widely used in mining tools, steel rolling rollers and cemented carbide stamping dies.

[0004] Mild ball milling is a method for preparing ultra-coarse cemented carbide based on the improvement of wet process. Due to its simple preparation process, it has been widely used in industrial production. However, the preparation process is prone to uneven metallographic structure. The short mild ball milling time and low mixing intensity may lead to uneven composition or structural defects, resulting in poor alloy performance.

[0005] Therefore, how to prepare an ultra-coarse-grained tungsten-cobalt cemented carbide with high hardness and good toughness is a technical problem that needs to be solved at present. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide to solve the problems raised in the background technology.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A method for preparing ultra-coarse-grained tungsten-cobalt cemented carbide comprises the following steps:

[0009] Step S1, prepare the following raw materials in parts by weight: 9-12 parts of cobalt powder, 105-115 parts of super coarse tungsten carbide, 12-16 parts of reinforcing component, 6-8 parts of anti-wear toughening agent, 1.5-3.1 parts of paraffin wax, and 28-52 parts of anhydrous ethanol;

[0010] Step S2, preparation of a mixture: adding ultra-coarse tungsten carbide, cobalt powder, reinforcing components, anti-wear toughening agents, paraffin wax and anhydrous ethanol to a rolling ball mill by weight, wet grinding for 8-24 hours, and vacuum drying to obtain a mixture, wherein the ball-to-material ratio of cemented carbide grinding balls to solid raw materials is 1:1-3:1. In the above process, paraffin wax is used as a binder, anhydrous ethanol is used as a solvent, and ultra-coarse tungsten carbide and cobalt powder are used as base materials, and the mixture is obtained by wet grinding process;

[0011] Step S3, granulation treatment: the mixed material prepared in step S2 is passed through an 80-mesh sieve, and then placed in a granulator and rolled for 1-3 minutes for granulation treatment;

[0012] Step S4, pressing: pressing the mixed material granulated in step S2 into a compact;

[0013] Step S5, sintering: the compact prepared in step S3 is pressurized and sintered into an ultra-coarse-grained tungsten-cobalt cemented carbide.

[0014] Furthermore, in step S2, the Fisher grain size (Fsss grain size) of the ultra-coarse tungsten carbide powder is 25-27 μm.

[0015] Furthermore, in step S4, the pressing pressure is 150-300 MPa.

[0016] Furthermore, in step S5, the pressed green sheet is sintered under overpressure conditions, and the sintering temperature is controlled at 1760-1820°C. During sintering, the temperature is first increased to 350-420°C at a heating rate of 6-8°C / min under vacuum, and kept warm for 10-20min, and then increased to 1450-1550°C at a heating rate of 12-16°C / min, and kept warm in vacuum for 15-25min, and the pressure is increased to 10-50MPa at a rate of 5-7MPa / min. At the same time, the temperature is increased to 1760-1820°C at a heating rate of 18-20°C / min, and then the pressure is increased to 80Mpa at a pressure increase rate of 5-7MPa / min, and the heat treatment is carried out for 2-3h.

[0017] Furthermore, the preparation method of the reinforcing component comprises the following steps:

[0018] Step B1, dissolving chitosan in an acetic acid aqueous solution with a mass fraction of 1%, ultrasonically dispersing for 20-40 minutes to obtain a dispersion, then dripping a polyvinyl alcohol solution with a mass concentration of 0.1 mg / L, and controlling the dripping to be completed within 30 minutes. After the dripping is completed, stirring is continued for 1-2 hours, and then modified niobium carbide is added, the temperature is raised to 65-75° C., and stirring is continued for 2-4 hours to obtain a reaction solution, wherein the amount ratio of chitosan, acetic acid aqueous solution, polyvinyl alcohol solution and modified niobium carbide is 1-2g:40-60mL:25-35mL:3.5-4.5g;

[0019] Step B2, placing the reaction solution into a centrifugal spray dryer for spray drying, controlling the air inlet temperature: 250-350°C, the air outlet temperature: 150°C, the rotation speed: 30000rpm, and the flow rate: 30mL / min, to obtain a dry component;

[0020] Step B3, the dried component is roasted at 500-600°C for 30-40 minutes in a nitrogen protective atmosphere, and then the temperature is raised to 850-1000°C, and reduced and carbonized for 80-100 minutes in a mixed gas condition of hydrogen and methane in a volume ratio of 3:1 to obtain a reinforcement component.

[0021] Furthermore, the preparation method of modified niobium carbide comprises the following steps:

[0022] The niobium carbide is placed at 100°C for drying for 0.5-1h, then ultrasonically mixed with deionized water, anhydrous ethanol and KH-550 for 30min, stirred at room temperature for reaction for 6-8h, centrifuged, and the precipitate is washed and dried to obtain modified niobium carbide, wherein the amount ratio of niobium carbide, deionized water, anhydrous ethanol and KH-550 is 5g:12mL:25-30mL:0.4-0.6mL. In the above reaction process, the niobium carbide is first treated with KH-550 to obtain modified niobium carbide containing amino groups.

[0023] Furthermore, the preparation method of the anti-wear toughening agent comprises the following steps:

[0024] Step A1, ultrasonically dispersing nano-alumina in a phosphoric acid solution with a mass fraction of 50-60%, heating to 110-120° C., stirring and reacting for 2-4 hours, to obtain component A;

[0025] The dosage ratio of nano-alumina to 50-60% phosphoric acid solution is 4-6 g: 36-44 mL;

[0026] Step A2, mixing nano zinc oxide, nano magnesium oxide, nano zirconium oxide and modified silica sol uniformly to obtain component B, wherein the amount ratio of nano zinc oxide, nano magnesium oxide, nano zirconium oxide and modified silica sol is 10-12g: 2.5-3g: 5-6g: 2.5-3.5mL;

[0027] Step A3, adding component A to component B, stirring evenly, to obtain an anti-wear toughening agent, wherein the amount ratio of component A to component B is 8-10 mL: 2-2.5 g.

[0028] Furthermore, the preparation method of the modified silica sol comprises the following steps:

[0029] Add tetraethyl orthosilicate to anhydrous ethanol, heat to 25-35°C, add 10%wt hydrochloric acid solution dropwise while stirring to adjust the pH value to 4-5, after adding, stir and react for 2h, add modifier, heat to 45-55°C and stir and react for 4-6h, cool to room temperature to obtain modified silica sol, wherein the amount ratio of tetraethyl orthosilicate, anhydrous ethanol and modifier is 16-18mL:6.7-7.7mL:2-4g, in the above reaction process, tetraethyl orthosilicate is used as a precursor, and the modifier and tetraethyl silicate undergo hydrolysis and condensation reaction under acidic conditions to obtain modified silica sol.

[0030] Furthermore, the preparation method of the modifier comprises the following steps:

[0031] Add vinyl phosphate and chloroplatinic acid catalyst to isopropanol, heat to 35-45°C, stir evenly, and add 1,1,3,3-tetramethyldisiloxane dropwise while stirring, and control the dripping to be completed within 30 minutes. After the dripping is completed, heat to reflux, continue to stir and react for 6-8 hours. After the reaction is completed, cool to room temperature, and remove the solvent by rotary evaporation to obtain a modifier, wherein the amount of vinyl phosphate, chloroplatinic acid catalyst, isopropanol and 1,1,3,3-tetramethyldisiloxane is 2-4g: 0.01-0.02mL: 55-75mL: 4.4-8.6mL. In the above reaction process, with isopropanol as solvent, the unsaturated double bond on the vinyl phosphate and the active hydrogen on the 1,1,3,3-tetramethyldisiloxane undergo a silylation reaction to obtain a modifier, and the structural formula of the modifier is shown below;

[0032]

[0033] Furthermore, the mass fraction of chloroplatinic acid in the chloroplatinic acid catalyst is 2%.

[0034] Compared with the prior art, the present invention has the following beneficial effects: In order to solve the problems existing in the prior art, the present invention provides an ultra-coarse-grained tungsten-cobalt cemented carbide. In its preparation process, two aspects are taken into consideration. First, a reinforcing component is added. The reinforcing component contains niobium carbide. On the one hand, it is dissolved in the cobalt phase in a solid solution form during the sintering process, affecting the dissolution and reprecipitation process of tungsten in cobalt, changing the morphology of tungsten carbide grains, so that a large proportion of tungsten carbide grains in the alloy are lath-shaped, and the lath-shaped tungsten carbide grains have a high aspect ratio and better flexibility, thereby improving the toughness of the alloy phase. On the other hand, the KH-550 coated on the modified niobium carbide can chemically bond with the hydroxyl groups on chitosan and polyvinyl alcohol to improve its dispersibility. At the same time, the compound liquid of chitosan and polyvinyl alcohol has excellent adhesion, and can couple with the tungsten carbide and cobalt alloy hard units to form a soft-hard coupling. The rough alloy structure is improved to improve the toughness of the alloy; secondly, an anti-wear toughening agent is added. The anti-wear toughening agent is prepared from an inorganic nano-metal substrate, a phosphoric acid solution and a modified silica sol. The inorganic nano-metal substrate has good wear resistance. The presence of the phosphoric acid group can improve the bonding performance of the group, improve the dispersion uniformity of the substrate, and further improve the toughness of the material. The modified silica sol is prepared by modifying tetraethyl orthosilicate with a modifier. The modifier contains a phosphate group and a siloxane group. The phosphate group has a good lubricating effect and can enhance the wear resistance of plastic parts. The presence of siloxane can give play to the good stability of the silicon element itself. The silica sol itself has good adhesion. It dehydrates at high temperature to form an inorganic silicon oxygen chain network macromolecule. The polyvinyl alcohol in the reinforcing component will decompose under high temperature sintering to form a carbon network structure. Through their joint action, the toughness and hardness of the alloy are improved together. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] Preferably, this embodiment provides a method for preparing modified niobium carbide, comprising the following steps:

[0038] 5 g of niobium carbide was dried at 100° C. for 0.75 h, then ultrasonically mixed with 12 mL of deionized water, 27.5 mL of anhydrous ethanol and 0.5 mL of KH-550 for 30 min, stirred at room temperature for 7 h, centrifuged, and the precipitate was washed and dried to obtain modified niobium carbide.

[0039] Example 2

[0040] Preferably, this embodiment provides a method for preparing a reinforcing component, comprising the following steps:

[0041] Step B1, dissolving 1.5 g of chitosan in 50 mL of 1% acetic acid aqueous solution, ultrasonically dispersing for 30 min to obtain a dispersion, then dripping 30 mL of a polyvinyl alcohol solution with a mass concentration of 0.1 mg / L, and controlling the dripping to be completed within 30 min. After the dripping is completed, stirring is continued for 1.5 h, and then 4 g of the modified niobium carbide prepared in Example 1 is added, the temperature is raised to 70° C., and stirring is continued for 3 h to obtain a reaction solution;

[0042] Step B2, placing the reaction solution in a centrifugal spray dryer for spray drying, controlling the air inlet temperature to 300°C, the air outlet temperature to 150°C, the rotation speed to 30000rpm, and the flow rate to 30mL / min, to obtain a dry component;

[0043] Step B3, the dried component is baked at 550° C. for 35 min in a nitrogen protective atmosphere, and then the temperature is raised to 925° C., and reduced and carbonized for 90 min in a mixed gas condition of hydrogen and methane in a volume ratio of 3:1 to obtain a reinforced component.

[0044] Example 3

[0045] Preferably, this embodiment provides a method for preparing a modifier, comprising the following steps:

[0046] Add 3g of vinyl phosphate and 0.015mL of chloroplatinic acid catalyst to 65mL of isopropanol, heat to 40°C, stir evenly, add 6.5mL of 1,1,3,3-tetramethyldisiloxane dropwise while stirring, and control the addition to be completed within 30min. After the addition is completed, heat to reflux and continue stirring to react for 7h. After the reaction is completed, cool to room temperature and remove the solvent by rotary evaporation to obtain a modifier.

[0047] Example 4

[0048] Preferably, this embodiment provides a method for preparing a modified silica sol, comprising the following steps:

[0049] 17 mL of ethyl orthosilicate was added to anhydrous ethanol, and the temperature was raised to 30°C. 7 mL of 10% wt hydrochloric acid solution was added dropwise while stirring to adjust the pH value to 4.5. After the addition was completed, the mixture was stirred for 2 h. 3 g of the modifier prepared in Example 3 was added, the temperature was raised to 50°C, and the mixture was stirred for 5 h. The mixture was cooled to room temperature to obtain a modified silica sol.

[0050] Example 5

[0051] Preferably, this embodiment provides a method for preparing an anti-wear toughening agent, comprising the following steps:

[0052] Step A1, ultrasonically disperse 5 g of nano-alumina in 40 mL of a 55% phosphoric acid solution, heat to 115° C., and stir for 3 h to obtain component A;

[0053] Step A2, 11 g of nano zinc oxide, 2.75 g of nano magnesium oxide, 5.5 g of nano zirconium oxide and 3 mL of the modified silica sol prepared in Example 4 were uniformly mixed to obtain component B;

[0054] Step A3: Add 9 mL of component A to 2.25 g of component B and stir evenly to obtain an anti-wear toughening agent.

[0055] Example 6

[0056] The present embodiment provides a method for preparing an ultra-coarse grain tungsten-cobalt cemented carbide, comprising the following steps: Step S1, preparing the following raw materials in parts by weight: 9 parts of cobalt powder, 105 parts of ultra-coarse tungsten carbide, 12 parts of the reinforcing component prepared in Example 2, 6 parts of the anti-wear toughening agent prepared in Example 5, 1.5 parts of paraffin wax, and 28 parts of anhydrous ethanol;

[0057] Step S2, preparation of a mixture: adding ultra-coarse tungsten carbide, cobalt powder, reinforcing component, anti-wear toughening agent, paraffin wax and anhydrous ethanol to a rolling ball mill by weight, wet grinding for 16 hours, and vacuum drying to obtain a mixture, wherein the ball-to-material ratio of cemented carbide grinding balls to solid raw materials is 1:1;

[0058] Step S3, pressing: pressing the mixed material granulated in step S2 into a compact at 200 MPa;

[0059] Step S4, sintering: the pressed green body prepared in step S3 is sintered into an ultra-coarse-grained WC-Co cemented carbide. During sintering, the temperature is gradually increased to 350°C at a heating rate of 6°C / min under vacuum, and the temperature is kept for 10 minutes. Then, the temperature is gradually increased to 1450°C at a heating rate of 12°C / min, and the vacuum is kept for 15 minutes. Then, the pressure is increased to 10MPa at a rate of 5MPa / min. At the same time, the temperature is gradually increased to 1760°C at a heating rate of 18°C / h, and the pressure is increased to 80Mpa at a pressure increase rate of 5MPa / min, and the temperature is kept for 2 hours.

[0060] Example 7

[0061] This embodiment provides a method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide, comprising the following steps:

[0062] Step S1, prepare the following raw materials in parts by weight: 10.5 parts of cobalt powder, 110 parts of ultra-coarse tungsten carbide, 14 parts of the reinforcing component prepared in Example 2, 7 parts of the anti-wear toughening agent prepared in Example 5, 2.3 parts of paraffin wax, and 40 parts of anhydrous ethanol;

[0063] Step S2, preparation of a mixture: adding ultra-coarse tungsten carbide, cobalt powder, reinforcing component, anti-wear toughening agent, paraffin wax and anhydrous ethanol to a rolling ball mill by weight, wet grinding for 16 hours, and vacuum drying to obtain a mixture, wherein the ball-to-material ratio of cemented carbide grinding balls to solid raw materials is 2:1;

[0064] Step S3, granulation treatment: the mixed material prepared in step S2 is passed through an 80-mesh sieve, and then placed in a granulator and rolled for 2 minutes for granulation treatment;

[0065] Step S4, pressing: pressing the mixed material granulated in step S2 into a compact at 275 MPa;

[0066] Step S5, sintering: sinter the compact prepared in step S3 into an ultra-coarse-grained tungsten-cobalt cemented carbide. During sintering, the temperature is gradually increased to 385°C at a heating rate of 7°C / min under vacuum, and kept warm for 15 minutes. The temperature is then gradually increased to 1500°C at a heating rate of 14°C / min, and kept warm in vacuum for 20 minutes. The pressure is then increased to 30MPa at a rate of 6MPa / min. At the same time, the temperature is gradually increased to 1790°C at a heating rate of 19°C / h / h, and the pressure is then increased to 80Mpa at a pressure increase rate of 6MPa / min, and kept warm for 2.5 hours.

[0067] Example 8

[0068] This embodiment provides a method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide, comprising the following steps:

[0069] Step S1, prepare the following raw materials by weight: 12 parts of cobalt powder, 115 parts of super coarse tungsten carbide, 16 parts of reinforcing component, 8 parts of anti-wear toughening agent, 3.1 parts of paraffin wax, and 52 parts of anhydrous ethanol;

[0070] Step S2, preparation of a mixture: adding, by weight, ultra-coarse tungsten carbide, cobalt powder, the reinforcing component prepared in Example 2, the anti-wear toughening agent prepared in Example 5, paraffin wax and anhydrous ethanol into a rolling ball mill, wet-milling for 24 hours, and vacuum drying to obtain a mixture, wherein the ball-to-material ratio of cemented carbide grinding balls to solid raw materials is 3:1;

[0071] Step S3, granulation treatment: the mixed material prepared in step S2 is passed through an 80-mesh sieve, and then placed in a granulator and rolled for 3 minutes for granulation treatment;

[0072] Step S4, pressing: pressing the mixed material granulated in step S2 into a compact at 350 MPa;

[0073] Step S5, sintering: the pressed green sheet prepared in step S3 is sintered into an ultra-coarse-grained tungsten-cobalt cemented carbide. During sintering, the temperature is first increased to 420°C at a heating rate of 8°C / min under vacuum, and kept warm for 20 minutes. Then, the temperature is increased to 1550°C at a heating rate of 16°C / min, and the vacuum is kept warm for 25 minutes. Then, the pressure is increased to 50MPa at a rate of 7MPa / min. At the same time, the temperature is increased to 1820°C at a heating rate of 20°C / h, and then the pressure is increased to 80Mpa at a pressure increase rate of 7MPa / min, and the heat preservation is carried out for 3 hours.

[0074] Comparative Example 1

[0075] The modified niobium carbide in Example 2 is removed, and the other raw materials and preparation process remain unchanged. The prepared material is then replaced with the reinforcing component in Example 7, and the other raw materials and preparation process remain unchanged.

[0076] Comparative Example 2

[0077] The polyvinyl alcohol solution in Example 2 is removed, and the other raw materials and preparation process remain unchanged. The prepared substance is then replaced with the reinforcing component in Example 7, and the other raw materials and preparation process remain unchanged.

[0078] Comparative Example 3

[0079] The reinforcing components in Example 7 were removed, and the remaining raw materials and preparation process remained unchanged.

[0080] Comparative Example 4

[0081] The modifier in Example 4 is removed, and the other raw materials and preparation process remain unchanged. The prepared substance is then replaced with the modified silica sol in Example 5, and the other raw materials and preparation process remain unchanged. The prepared substance is then replaced with the anti-wear toughening agent in Example 7, and the other raw materials and preparation process remain unchanged.

[0082] Comparative Example 5

[0083] The anti-wear toughening agent in Example 7 was removed, and the other raw materials and preparation process remained unchanged.

[0084] Performance Testing

[0085] The properties of the ultra-coarse-grained WC-Co cemented carbides prepared in Examples 4-6 and Comparative Examples 1-5 were tested. The Vickers hardness was measured using a HV-50A Vickers hardness tester, and the fracture toughness was calculated based on the indentation crack length. The coarse-grained grain size was determined using the method in GB / T6394-2017 "Method for Determination of Average Grain Size of Metals". The specific test results are shown in Table 1:

[0086] Table 1

[0087]

[0088] It can be seen from the data in Table 1 that, compared with Comparative Examples 1-5, the ultra-coarse-grained WC-Co cemented carbides prepared in Examples 4-6 have larger grain sizes, higher hardness and better toughness.

[0089] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing ultra-coarse-grained tungsten-cobalt cemented carbide, characterized in that: The following steps are involved: Step S1, prepare the following raw materials in parts by weight: 9-12 parts of cobalt powder, 105-115 parts of super coarse tungsten carbide, 12-16 parts of reinforcing component, 6-8 parts of anti-wear toughening agent, 1.5-3.1 parts of paraffin wax, and 28-52 parts of anhydrous ethanol; Step S2, preparation of a mixture: adding ultra-coarse tungsten carbide, cobalt powder, anti-wear toughening agent, paraffin and anhydrous ethanol to a rolling ball mill by weight, wet grinding for 8-24 hours, and vacuum drying to obtain a mixture, wherein the ball-to-material ratio of cemented carbide grinding balls to solid raw materials is 1-3:1, and in the above process, paraffin is used as a binder and anhydrous ethanol is used as a solvent; Step S3, granulation treatment: the mixed material prepared in step S2 is passed through an 80-mesh sieve, and then placed in a granulator and rolled for 1-3 minutes for granulation treatment; Step S4, pressing: pressing the mixed material granulated in step S2 into a compact; Step S5, sintering: pressurizing and sintering the compact prepared in step S3 into an ultra-coarse-grained tungsten-cobalt cemented carbide; The preparation method of the reinforcing component comprises the following steps: Step B1, dissolving chitosan in an acetic acid aqueous solution with a mass fraction of 1%, ultrasonically dispersing for 20-40 minutes to obtain a dispersion, and then dripping a polyvinyl alcohol solution with a mass concentration of 0.1 mg / L, and controlling the dripping to be completed within 30 minutes. After the dripping is completed, stirring is continued for 1-2 hours, and then modified niobium carbide is added, the temperature is raised to 65-75° C., and stirring is continued for 2-4 hours to obtain a reaction solution; Step B2, placing the reaction solution into a centrifugal spray dryer for spray drying, controlling the air inlet temperature: 250-350°C, the air outlet temperature: 150°C, the rotation speed: 30000rpm, and the flow rate: 30mL / min, to obtain a dry component; Step B3, the dried component is baked at 500-600°C for 30-40 minutes in a nitrogen protective atmosphere, and then the temperature is increased to 850-1000°C, and reduced and carbonized for 80-100 minutes in a mixed gas condition of hydrogen and methane with a volume ratio of 3:1 to obtain a reinforcement component.

2. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 1, characterized in that: The preparation method of the modified niobium carbide comprises the following steps: The niobium carbide is dried at 100° C. for 0.5-1 h, then ultrasonically mixed with deionized water, anhydrous ethanol and KH-550 for 30 min, stirred at room temperature for 6-8 h, centrifuged, and the precipitate is washed and dried to obtain modified niobium carbide.

3. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 1, characterized in that: The preparation method of the anti-wear toughening agent comprises the following steps: Step A1, ultrasonically disperse aluminum oxide in a phosphoric acid solution with a mass fraction of 50-60%, heat to 110-120° C., stir and react for 2-4 hours to obtain component A; Step A2, uniformly mixing zinc oxide, magnesium oxide, zirconium oxide and modified silica sol to obtain component B; Step A3, adding component A to component B, stirring evenly, to obtain an anti-wear toughening agent.

4. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 1, characterized in that: The preparation method of the modified silica sol comprises the following steps: Add ethyl orthosilicate to anhydrous ethanol, heat to 25-35°C, add 10%wt hydrochloric acid solution dropwise while stirring to adjust the pH value to 4-5, after adding, stir and react for 2h, add modifier, heat to 45-55°C, stir and react for 4-6h, cool to room temperature to obtain modified silica sol.

5. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 1, characterized in that: The preparation method of the modifier comprises the following steps: Add vinyl phosphate and chloroplatinic acid catalyst to isopropanol, heat to 35-45°C, stir evenly, add 1,1,3,3-tetramethyldisiloxane dropwise while stirring, and control the dripping to be completed within 30 minutes. After the dripping is completed, heat to reflux and continue stirring to react for 6-8 hours. After the reaction is completed, cool to room temperature, and remove the solvent by rotary evaporation to obtain a modifier.

6. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 1, characterized in that: In the step B1, the usage ratio of chitosan, acetic acid aqueous solution, polyvinyl alcohol solution and modified niobium carbide is 1-2 g: 40-60 mL: 25-35 mL: 3.5-4.5 g.

7. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 2, characterized in that: The usage ratio of the niobium carbide, deionized water, anhydrous ethanol and KH-550 is 5g:12mL:25-30mL:0.4-0.6mL.

8. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 3, characterized in that: In the step A1, the dosage ratio of aluminum oxide and phosphoric acid solution with a mass fraction of 50-60% is 4-6 g: 36-44 mL, in the step A2, the dosage ratio of zinc oxide, magnesium oxide, zirconium oxide and modified silica sol is 10-12 g: 2.5-3 g: 5-6 g: 2.5-3.5 mL, and in the step A3, the dosage ratio of component A and component B is 8-10 mL: 2-2.5 g.

9. The method for preparing an ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 4, characterized in that: The usage ratio of the tetraethyl orthosilicate, anhydrous ethanol and the modifier is 16-18 mL: 6.7-7.7 mL: 2-4 g.

10. The method for preparing ultra-coarse-grained tungsten-cobalt cemented carbide according to claim 5, characterized in that: The usage of the vinyl phosphate, chloroplatinic acid catalyst, isopropanol and 1,1,3,3-tetramethyldisiloxane is 2-4g: 0.01-0.02mL: 55-75mL: 4.4-8.6mL.

Citation Information

Patent Citations

  • Method for preparing high-tenacity super-coarse-grained tungsten and cobalt hard alloy

    CN101985717A

  • Preparation method for high-strength and high-hardness nanocrystalline tungstate-cobalt hard alloy

    CN102994792A

  • Rare-earth-added ultra-fine grain high-toughness WC-10Co hard alloy material and preparation method

    CN111088450A

  • Composition for preparing low-cobalt extremely-coarse-grain hard alloy, low-cobalt extremely-coarse-grain hard alloy and preparation method and application of low-cobalt extremely-coarse-grain hard alloy

    CN115584423A

Cited By

  • Pyraclostrobin thioneb water dispersible granule and preparation process thereof

    CN119547779A

  • Ultra-coarse grain WC-Co hard alloy and preparation method thereof

    CN120138413A

  • Ultra-coarse-grained WC-Co cemented carbide and preparation method thereof

    CN120138413B

  • High-strength hard alloy cutter base material and preparation method thereof

    CN120138414A