A kind of anticorrosive coating based on modified graphene and preparation method thereof
By thermal reduction and modification of graphite oxide, modified graphene is prepared with good dispersion, combined with modified aqueous epoxy resin, the problem of insufficient adhesion and corrosion resistance of single-component coatings is solved, and the further development is achieved Strong anti-corrosion performance and wider application.
Patent Information
- Application Number
- CN202411244598.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The adhesion and corrosion resistance of existing single-component coatings are insufficient, and the insolubleness and accumulation of graphene in water and organic solvents lead to difficulty in uniform distribution in anticorrosion coatings, limiting the anticorrosion performance.
By thermal reduction of graphite oxide, more reduced graphene oxide is obtained, and modified to prepare modified graphene A and modified graphene B with better dispersion, combined with modified aqueous rings Oxygen resin and other components form a uniformly distributed anticorrosion coating, enhancing adhesion and corrosion resistance.
It significantly improves the adhesion, corrosion resistance and corrosion resistance of the paint, expands the application prospects, and further improves the corrosion resistance after soaking.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and in particular to an anti-corrosion coating based on modified graphene and a preparation method thereof. Background Art
[0002] Commonly used metal protection technologies include cathodic protection, corrosion inhibitor protection, metal plating and surface organic coating. Among them, surface organic coating is the most commonly used, most effective and the highest proportion of anti-corrosion methods. Therefore, it is a hot and necessary technical issue to study the mechanism of metal corrosion and seek effective organic anti-corrosion coatings to protect metals to slow down the rate of metal corrosion and reduce the harm caused by corrosion. Depending on whether other ingredients need to be added during use, coatings can be divided into single-component coatings and multi-component coatings. Compared with multi-component coatings, single-component coatings are easier to store and more convenient to use. Therefore, single-component coatings have broader application prospects. However, the performance of single-component coatings in the prior art in terms of adhesion and corrosion resistance still needs to be improved.
[0003] As an extremely thin two-dimensional nanomaterial, graphene has excellent barrier and shielding properties. Therefore, the coating prepared using graphene coating not only has excellent shielding properties, can block corrosion factors such as oxygen and water molecules from reaching the surface of the metal substrate, but also has excellent thermal, electrical and mechanical properties. However, graphene itself is inert and is easily affected by van der Waals forces and is prone to irreversible accumulation, making it difficult to dissolve in water and commonly used organic solvents, and even more difficult to compound with organic or inorganic materials. Therefore, in the field of using graphene to prepare anti-corrosion coatings, how to evenly distribute graphene materials in anti-corrosion coatings to extend the contact path between corrosion factors such as water and oxygen molecules and the protected substrate and reduce the electrochemical corrosion reaction caused by accumulation, thereby improving the anti-corrosion performance of the coating is of great significance.
[0004] The prior art often improves the anti-corrosion performance of the coating by modifying graphene to reduce its agglomeration in the film-forming carrier and make its distribution more uniform, thereby effectively extending the contact path between corrosion factors such as water and oxygen molecules and the protected substrate. For example, the patent document CN115181478B discloses a graphene-modified anti-corrosion coating, a preparation method thereof and its application. The graphene-modified anti-corrosion coating of the invention includes a first component and a second component; the first component includes the following ingredients: epoxy resin, reduced graphene oxide modified by silane coupling agent, nano-ceramic powder, defoamer and leveling agent; the second component includes the following ingredients: amine curing agent, defoamer and leveling agent. However, this method cannot prevent all corrosion factors such as oxygen and water molecules from reaching the surface of the metal substrate, so the anti-corrosion ability is very limited. In addition, this type of multi-component coating is inconvenient to use and store.
[0005] Therefore, according to the above-mentioned related technologies, it is urgent to develop an anti-corrosion coating based on modified graphene and a preparation method thereof. Summary of the invention
[0006] In view of this, the purpose of the present invention is to propose an anti-corrosion coating based on modified graphene and a preparation method thereof, so as to alleviate the problem of poor anti-corrosion effect of coatings in the prior art.
[0007] Based on the above objectives, the present invention provides an anti-corrosion coating based on modified graphene and a preparation method thereof.
[0008] A method for preparing an anti-corrosion coating based on modified graphene specifically comprises the following steps:
[0009] Step S1. Add modified graphene B and dispersant NNO to the modified waterborne epoxy resin in sequence, stir at 75-80° C. and 300-350 r / min for 15-30 min to obtain a premixed coating;
[0010] Step S2. Add T31 curing agent, tributyl phosphate and leveling agent to the premixed coating, stir at 300-350 r / min for 15-30 min to obtain an anti-corrosion coating based on modified graphene;
[0011] The modified waterborne epoxy resin is prepared from water, sodium carboxymethyl cellulose, reduced graphene oxide and waterborne epoxy resin;
[0012] The modified graphene B is prepared from 2,6-diaminopyridine, water and reduced graphene oxide;
[0013] The reduced graphene oxide is obtained by subjecting graphite oxide to thermal reduction treatment.
[0014] Preferably, the mass ratio of the modified waterborne epoxy resin, modified graphene B and dispersant NNO in step S1 is 99.2-101.25:0.1-0.15:1-1.5; the mass ratio of the premixed coating, T31 curing agent, tributyl phosphate and leveling agent in step S2 is 100.3-102.9:4-7:0.1-0.5:0.5-1.
[0015] Preferably, the leveling agent in step S2 is any one of H633 leveling agent and H550 leveling agent.
[0016] Preferably, the preparation method of the modified waterborne epoxy resin in step S1 is as follows:
[0017] Step A1. First, sodium carboxymethyl cellulose was added to water, and stirred at 850-900 r / min for 45-60 min, and then reduced graphene oxide was added, ultrasonicated for 2.5-3 h, purified by ultrafiltration, and then dried in a vacuum at 75-80 ° C for 24-25 h to obtain graphene A;
[0018] Step A2. Add water to the waterborne epoxy resin and stir evenly, then add the modified graphene A and mix, and stir at a speed of 300-350 r / min for 15-20 min to obtain a modified waterborne epoxy resin.
[0019] Preferably, the mass ratio of water, sodium carboxymethyl cellulose and reduced graphene oxide in step A1 is 83-84:0.7-1.1:13.5-15; the mass ratio of water-based epoxy resin, water and modified graphene A in step A2 is 40-41:59-60:0.2-0.25.
[0020] Preferably, the preparation method of the modified graphene in step S1 is as follows:
[0021] Step B1. Add reduced graphene oxide to water and perform ultrasonic dispersion treatment for 30-45 min to obtain a graphene dispersion;
[0022] Step B2. Add 2,6-diaminopyridine to water and stir evenly, then add graphene dispersion, stir at 75-80°C for 30-35 minutes, then dry at 75-80°C, grind, and obtain modified graphene B.
[0023] Preferably, the mass ratio of water to reduced graphene oxide in step B1 is 90-100:0.2-0.25.
[0024] Preferably, the mass ratio of water, 2,6-diaminopyridine and graphene dispersion in step B2 is 18-20: 0.05-0.1: 90-100.
[0025] Preferably, the preparation method of the reduced graphene oxide is as follows:
[0026] 20-23 g of graphite oxide was placed in a corundum crucible, and the temperature was gradually raised to 785-800° C. in a nitrogen atmosphere, and kept at 785-800° C. for 10-15 min, and then cooled to 35-50° C. to obtain reduced graphene oxide.
[0027] An anti-corrosion coating based on modified graphene, wherein the anti-corrosion coating is prepared by the preparation method according to any one of claims 1 to 9.
[0028] Beneficial effects of the present invention:
[0029] The invention provides an anti-corrosion coating based on modified graphene and a preparation method thereof. The invention obtains reduced graphene oxide with more epoxy groups and larger specific surface area by thermally reducing graphite oxide, and then modifies the reduced graphene oxide to prepare modified graphene A and modified graphene B with better dispersibility; then the modified graphene A is used to modify waterborne epoxy resin, so that the adhesion and anti-corrosion ability of the coating are greatly improved; and after the modified graphene B is added, it interacts with other components and is very evenly dispersed in the coating, so that the adhesion and anti-corrosion ability of the coating are further improved. Compared with the prior art, the anti-corrosion coating based on modified graphene prepared by the invention has stronger anti-corrosion ability and wider application prospects. DETAILED DESCRIPTION
[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0031] The sources and properties of some of the raw materials used in the present invention are as follows:
[0032] Graphite oxide was purchased from Changzhou Sixth Element Materials Technology Co., Ltd., 15-35 μm; water-based epoxy resin was purchased from Shenzhen Yoshida Chemical Co., Ltd.; dispersant NNO was purchased from Shanghai Aladdin Reagent Co., Ltd., CAS: 36290-04-7; T31 curing agent was purchased from Guangdong Tu'an Anticorrosion Technology Co., Ltd.; tributyl phosphate was purchased from Shanghai Aladdin Reagent Co., Ltd., CAS: 126-73-8; H633 leveling agent was purchased from Suzhou Senfida Chemical Co., Ltd., CAS: 67762-85-0; H850 leveling agent was purchased from Jiangxi Haiduo Silicone Materials Co., Ltd., CAS: 157479-55-5; sodium carboxymethyl cellulose was purchased from Shanghai Aladdin Reagent Co., Ltd., CAS: 9004-32-4; 2,6-diaminopyridine was purchased from Shanghai Aladdin Reagent Co., Ltd., CAS: 141-86-6.
[0033] Example 1: A method for preparing an anti-corrosion coating based on modified graphene, the specific preparation method is as follows:
[0034] Step S1. 20 g of graphite oxide was placed in a corundum crucible, and the temperature was gradually raised to 785° C. in a nitrogen atmosphere, and kept at 785° C. for 10 min, and then cooled to 35° C. to obtain reduced graphene oxide;
[0035] Step S2. First, 83 g of water and 0.7 g of sodium carboxymethyl cellulose were added to a three-necked flask, stirred at 850 r / min for 45 min, and then 13.5 g of reduced graphene oxide was added, ultrasonically vibrated for 2.5 h, purified by ultrafiltration, and then dried in a vacuum at 75 ° C for 24 h to obtain modified graphene A;
[0036] Step S3. Add 59 g of water to 40 g of waterborne epoxy resin, stir evenly, then add 0.2 g of modified graphene A, stir at a speed of 300 r / min for 15 min to obtain a modified waterborne epoxy resin;
[0037] Step S4. Add 0.2 g of reduced graphene oxide to 90 g of water and perform ultrasonic dispersion treatment for 30 min to obtain a graphene dispersion;
[0038] Step S5. Add 0.05 g of 2,6-diaminopyridine to 18 g of water, stir evenly, then add 90 g of graphene dispersion, stir at 75 ° C for 30 min, and then dry at 75 ° C and grind to obtain modified graphene B;
[0039] Step S6. Add 0.1 g of modified graphene B and 1 g of dispersant NNO to 99.2 g of modified waterborne epoxy resin, stir at 75° C. and 300 r / min for 15 min to obtain a premixed coating;
[0040] Step S7. Add 4 g of T31 curing agent, 0.1 g of tributyl phosphate and 0.5 g of H633 leveling agent to 100.3 g of the premixed coating, and stir at 300 r / min for 15 min to obtain an anti-corrosion coating based on modified graphene;
[0041] Example 2: A method for preparing an anti-corrosion coating based on modified graphene, the specific preparation method is as follows:
[0042] Step S1. 21 g of graphite oxide was placed in a corundum crucible, and the temperature was gradually raised to 790° C. in a nitrogen atmosphere, and kept at 790° C. for 12 min, and then cooled to 40° C. to obtain reduced graphene oxide;
[0043] Step S2. First, 83.3 g of water and 0.8 g of sodium carboxymethyl cellulose were added to a three-necked flask, stirred at 870 r / min for 50 min, then 14 g of reduced graphene oxide was added, ultrasonicated for 2.7 h, purified by ultrafiltration, and then dried at 77 ° C under vacuum for 24.3 h to obtain modified graphene A;
[0044] Step S3. Add 59.3 g of water to 40.3 g of waterborne epoxy resin, stir evenly, then add 0.22 g of modified graphene A, stir at a speed of 320 r / min for 17 min, and obtain a modified waterborne epoxy resin;
[0045] Step S4. Add 0.22 g of reduced graphene oxide to 93 g of water and perform ultrasonic dispersion treatment for 35 min to obtain a graphene dispersion;
[0046] Step S5. Add 0.07 g of 2,6-diaminopyridine to 18.7 g of water, stir evenly, then add 93 g of graphene dispersion, stir at 77 ° C for 32 min, and then dry at 77 ° C and grind to obtain modified graphene B;
[0047] Step S6. 0.12 g of modified graphene B and 1.2 g of dispersant NNO were added to 99.52 g of modified waterborne epoxy resin in sequence, and stirred at 77° C. and 320 r / min for 20 min to obtain a premixed coating;
[0048] Step S7. Add 5 g of T31 curing agent, 0.3 g of tributyl phosphate and 0.7 g of H633 leveling agent to 100.84 g of the premixed coating, and stir at 320 r / min for 20 min to obtain an anti-corrosion coating based on modified graphene;
[0049] Example 3: A method for preparing an anti-corrosion coating based on modified graphene, the specific preparation method is as follows:
[0050] Step S1. 22 g of graphite oxide was placed in a corundum crucible, and the temperature was gradually raised to 795° C. in a nitrogen atmosphere, and kept at 795° C. for 14 min, and then cooled to 45° C. to obtain reduced graphene oxide;
[0051] Step S2. First, 83.6 g of water and 0.9 g of sodium carboxymethyl cellulose were added to a three-necked flask, stirred at 890 r / min for 55 min, then 14.5 g of reduced graphene oxide was added, ultrasonicated for 2.9 h, purified by ultrafiltration, and then dried at 79 ° C under vacuum conditions for 24.6 h to obtain modified graphene A;
[0052] Step S3. Add 59.6 g of water to 40.6 g of waterborne epoxy resin, stir evenly, then add 0.24 g of modified graphene A, stir at a speed of 340 r / min for 19 min to obtain a modified waterborne epoxy resin;
[0053] Step S4. Add 0.24 g of reduced graphene oxide to 96 g of water and perform ultrasonic dispersion treatment for 40 min to obtain a graphene dispersion;
[0054] Step S5. Add 0.09 g of 2,6-diaminopyridine to 19.5 g of water, stir evenly, then add 97 g of graphene dispersion, stir at 79 ° C for 34 min, and then dry at 79 ° C and grind to obtain modified graphene B;
[0055] Step S6. 0.14 g of modified graphene B and 1.4 g of dispersant NNO were added to 100.4 g of modified waterborne epoxy resin in sequence, and stirred at 78° C. and 340 r / min for 25 min to obtain a premixed coating;
[0056] Step S7. Add 6 g of T31 curing agent, 0.4 g of tributyl phosphate and 0.9 g of H550 leveling agent to 101.94 g of the premixed coating, and stir at 340 r / min for 25 min to obtain an anti-corrosion coating based on modified graphene;
[0057] Example 4: A method for preparing an anti-corrosion coating based on modified graphene, the specific preparation method is as follows:
[0058] Step S1. 23 g of graphite oxide was placed in a corundum crucible, and the temperature was gradually raised to 800° C. in a nitrogen atmosphere, and kept at 800° C. for 15 min, and then cooled to 50° C. to obtain reduced graphene oxide;
[0059] Step S2. First, 84 g of water and 1.1 g of sodium carboxymethyl cellulose were added to a three-necked flask, stirred at 900 r / min for 60 min, then 15 g of reduced graphene oxide was added, ultrasonicated for 3 h, purified by ultrafiltration, and then dried in a vacuum at 80 ° C for 25 h to obtain modified graphene A;
[0060] Step S3. Add 60 g of water to 41 g of waterborne epoxy resin, stir evenly, then add 0.25 g of modified graphene A, stir at a speed of 350 r / min for 20 min to obtain a modified waterborne epoxy resin;
[0061] Step S4. Add 0.25 g of reduced graphene oxide to 100 g of water and perform ultrasonic dispersion treatment for 45 min to obtain a graphene dispersion;
[0062] Step S5. Add 0.1 g of 2,6-diaminopyridine to 20 g of water, stir evenly, then add 100 g of graphene dispersion, stir at 80 ° C for 35 min, and then dry at 80 ° C and grind to obtain modified graphene B;
[0063] Step S6. 0.15 g of modified graphene B and 1.5 g of dispersant NNO were added to 101.25 g of modified waterborne epoxy resin in sequence, and stirred at 80° C. and 350 r / min for 30 min to obtain a premixed coating;
[0064] Step S7. Add 7 g of T31 curing agent, 0.5 g of tributyl phosphate and 1 g of H550 leveling agent to 102.9 g of the premixed coating, and stir at 350 r / min for 30 min to obtain an anti-corrosion coating based on modified graphene;
[0065] Comparative Example 1:
[0066] Compared with Example 1, this comparative example only replaces "reduced graphene oxide" with "graphene oxide", and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, an anti-corrosion coating based on modified graphene is obtained.
[0067] Comparative Example 2:
[0068] Compared with Example 1, this comparative example only replaces "modified graphene A" with "reduced graphene oxide", and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, an anti-corrosion coating based on modified graphene is obtained.
[0069] Comparative Example 3:
[0070] Compared with Example 1, this comparative example only replaces the "modified water-based epoxy resin" with the "water-based epoxy resin", and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, an anti-corrosion coating based on modified graphene is obtained.
[0071] Comparative Example 4:
[0072] Compared with Example 1, this comparative example only replaces "modified graphene B" with "reduced graphene oxide", and the remaining steps and parameters are the same, which will not be repeated in this comparative example. Finally, an anti-corrosion coating based on modified graphene is obtained.
[0073] Comparative Example 5:
[0074] Compared with Example 1, this comparative example only replaces "modified graphene A and modified graphene B" with "reduced graphene oxide", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally an anti-corrosion coating based on modified graphene is obtained.
[0075] Comparative Example 6:
[0076] Compared with Example 1, this comparative example replaces the "modified water-based epoxy resin" with the "water-based epoxy resin" and replaces the "modified graphene B" with the "reduced graphene oxide", and the remaining steps and parameters are the same, which will not be repeated in this comparative example, and finally an anti-corrosion coating based on modified graphene is obtained.
[0077] Comparative Example 7:
[0078] Compared with Example 1, this comparative example replaces "99.2g of modified water-based epoxy resin" with "99g of water-based epoxy resin" and replaces "0.1g of modified graphene B" with "0.2g of modified graphene A and 0.1g of modified graphene B". The remaining steps and parameters are the same and will not be repeated in this comparative example. Finally, an anti-corrosion coating based on modified graphene is obtained.
[0079] Performance Test:
[0080] Take 11 groups of steel plates with a size of 120 mm × 50 mm, remove the rust on the surface with 1200 mesh sandpaper, then use anhydrous ethanol to ultrasonically clean the steel plates, and blow dry them with a hair dryer for use; place the treated steel plates on the test bench, and use a wire rod coater with a specification of 100 μm (Oshiji Precision Tools Co., Ltd.) to apply the anti-corrosion coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 7 on each group of steel plates, respectively, with a wet film thickness of 100 μm; after coating, place the sample flat on the test bench, dry it at 25°C for 24 hours, and obtain an anti-corrosion coating sample, and perform performance tests on the prepared anti-corrosion coating sample:
[0081] Adhesion test:
[0082] Referring to the test standard of GB / T9286-2021 "Paint and Varnish - Scratching Test", place the anti-corrosion coating sample on a flat and hard operating table, and use a hundred-grid blade to evenly scratch in two directions perpendicular to each other. During this process, pay attention to even force and smooth scratching without shaking, and the scratching should penetrate the coating and touch the metal plate. After scratching, use a soft brush to gently wipe along the diagonal direction of the grid, and then stick the special 3M tape on the entire grid formed by the scratching. Press hard with your fingers to ensure that the tape is in good contact with the coating. When tearing off the tape, the tape should be at a 60° angle to the coating and tear off smoothly and quickly within 1s. The coating adhesion level is evaluated by observing the size of the tearing area, which is divided into 0-5 levels. The adhesion is strongest at level 0 and the worst at level 5. According to this test standard, the adhesion (level) test is carried out on the samples prepared with the anti-corrosion coatings prepared in Example 1-Example 4 and Comparative Example 1-Comparative Example 7;
[0083] Contact angle test:
[0084] Referring to the test standard GB / T30693-2014 "Measurement of the contact angle between plastic film and water", the anti-corrosion coating sample to be tested was tested using a water contact angle tester (OCA-25), the anti-corrosion coating sample was placed on the platform of the contact angle tester, and the contact angle between the sample surface and distilled water was measured. The result was read after the sample was in contact with the liquid to be tested for 30 seconds. Five different positions on the surface of the sample were taken, and the average value was taken as the contact angle (°) of the sample prepared with the anti-corrosion coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 7.
[0085] Corrosion resistance test:
[0086] Referring to the test standard of GB / T10125-2021 "Artificial Atmosphere Corrosion Test-Salt Spray Test", the anti-corrosion coating sample was edge-sealed with epoxy putty, and then placed in a salt spray test box (JAY-1127, Zhuhai Jiayi Testing Equipment Co., Ltd.), at 35°C, with a pH of 6.5-7.2 and a concentration of 5% sodium chloride solution for 24h salt spray and 24h drying cycle test, and sampling and observation were performed every 48h, and the test time for the appearance of red rust on each sample was recorded. The neutral salt spray test was terminated when the last sample appeared red rust; according to this test standard, the corrosion resistance (h) test was performed on the samples prepared with the anti-corrosion coatings prepared in Example 1-Example 4 and Comparative Example 1-Comparative Example 7;
[0087] Corrosion resistance test after immersion:
[0088] Referring to the test standard of GB / T10125-2021 "Artificial Atmosphere Corrosion Test-Salt Spray Test", the anti-corrosion coating sample was edge-sealed with epoxy putty, and then immersed in 5% sodium chloride for 7 days and then placed in a salt spray corrosion box (YWX-150, Changzhou National Testing Equipment Institute). At 35°C, a 24-hour salt spray and 24-hour drying cycle test was performed with a sodium chloride solution with a pH of 6.5-7.2 and a concentration of 5%, and samples were taken and observed every 48 hours, and the test time for the appearance of red rust on each sample was recorded. The neutral salt spray test was terminated when the last sample appeared red rust; according to this test standard, the samples prepared with the anti-corrosion coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 7 were immersed and then tested for corrosion resistance (h);
[0089] Impact resistance test:
[0090] Referring to the test standard of GB / T20624.2-2006 "Paints and varnishes - Rapid impact (impact resistance) test, Part 2: Drop hammer test (small area punch)", a paint film impact tester (TCJ-Ⅱ, Shanghai Leao Testing Instrument Co., Ltd.) with a weight of 1 kg was used to test the impact resistance (kg·m) of the samples prepared with the anti-corrosion coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 7;
[0091] Heat resistance test:
[0092] Referring to the test standard of GB / T1735-2009 "Paints and varnishes - Determination of heat resistance", the samples prepared with the anticorrosive coatings prepared in Examples 1 to 4 and Comparative Examples 1 to 7 were subjected to high temperature treatment for 24 hours at 125°C using an electric constant temperature blast drying oven (DHG-9140A, Shanghai Qixin Scientific Instrument Co., Ltd.), and then cooled to 25-30°C. Referring to the test standard of GB / T20624.2-2006 "Paints and varnishes - Rapid impact (impact resistance) test, Part II: Drop hammer test (small area punch)", a paint film impactor tester with a weight of 1 kg (TCJ-Ⅱ, Shanghai Leao Testing Instrument Co., Ltd.) was used to perform a heat resistance (kg·m) test, and the results are shown in Table 2;
[0093] Table 1 Summary of the amount of raw materials used in Examples 1 to 4 and Comparative Examples 1 to 7
[0094] project Graphene oxide / g Modified waterborne epoxy resin / g Modified graphene A / g Modified graphene B / g Example 1 0 99.20 0.20 0.10 Example 2 0 99.52 0.22 0.12 Example 3 0 100.40 0.24 0.14 Example 4 0 101.25 0.25 0.15 Comparative Example 1 13.7 99.20 0.20 0.10 Comparative Example 2 0 99.20 0 0.10 Comparative Example 3 0 0 0 0.10 Comparative Example 4 0 99.20 0.20 0 Comparative Example 5 0 99.20 0 0 Comparative Example 6 0 0 0 0 Comparative Example 7 0 0 0.20 0.10
[0095] Table 2 Performance test of samples of Example 1-Example 4 and Comparative Example 1-Comparative Example 7
[0096] project Adhesion / Grade Contact angle / ° Corrosion resistance / h Corrosion resistance after immersion / h Impact resistance / kg·m Heat resistance / kg·m Example 1 0 110.37 1584 1584 0.50 0.50 Example 2 0 109.79 1632 1632 0.55 0.50 Example 3 0 111.76 1680 1728 0.55 0.55 Example 4 0 110.78. 1680 1728 0.55 0.55 Comparative Example 1 0 95.77 1536 1488 0.45 0.40 Comparative Example 2 0 92.39 1488 1344 0.45 0.40 Comparative Example 3 1 86.56 1440 1200 0.40 0.30 Comparative Example 4 1 85.64 1536 1488 0.40 0.35 Comparative Example 5 1 82.67 1248 1008 0.35 0.25 Comparative Example 6 1 81.89 1104 720 0.30 0.20 Comparative Example 7 0 92.63 1488 1200 0.45 0.40
[0097] Data Analysis:
[0098] It can be seen from Table 2 that the anticorrosion coating based on modified graphene prepared by the present invention has better adhesion, corrosion resistance, immersion resistance, impact resistance and heat resistance, and a larger contact angle. The larger the contact angle, the lower the surface energy, that is, the anticorrosion coating prepared by the present invention also has a lower surface energy.
[0099] This may be because the present invention obtains reduced graphene oxide with more epoxy groups, larger specific surface area and high thermal conductivity by thermal reduction of graphite oxide, and then modifies the reduced graphene oxide to prepare modified graphene A and modified graphene B with better dispersibility; at the same time, the water-based epoxy resin is modified with modified graphene A, so that the adhesion, contact angle, corrosion resistance and impact resistance of the coating are greatly improved; and after the modified graphene B is added, it will interact with other components, disperse very evenly in the coating, and form stable complexes with iron ions or other ions in the metal matrix, so that the adhesion, corrosion resistance and heat resistance of the coating are further improved; when the coating is made into a coating and then immersed in water for a long time, the modified graphene B will also capture the electrons generated by the dissolution of the metal matrix, so that the iron ions form an iron oxide or ferroferric oxide passivation film on the surface of the metal group, which makes the corrosion resistance of the coating not only not decrease after immersion, but also slightly improve.
[0100] In Comparative Example 1, "reduced graphene oxide" is replaced by "graphene oxide". It can be seen from Table 2 that the corrosion resistance, contact angle, impact resistance and heat resistance are poorer than those in Example 1, and the corrosion resistance decreases more after immersion. This may be because compared with graphene oxide, the reduced graphene oxide prepared by the thermal reduction method of the present invention has a larger specific surface area and more epoxy groups to prepare modified graphene with a higher grafting degree; In Comparative Example 2, "modified graphene A" is replaced by "reduced graphene oxide". It can be seen from Table 2 that the contact angle, corrosion resistance, impact resistance and heat resistance are poorer than those in Example 1, and the corrosion resistance decreases more after immersion. This may be due to the fact that compared with graphene oxide, the reduced graphene oxide prepared by the thermal reduction method of the present invention has a larger specific surface area and more epoxy groups to prepare modified graphene with a higher grafting degree. It may be because the reduced graphene oxide has better dispersibility after being grafted with sodium carboxymethyl cellulose, and can react more fully with the water-based epoxy resin; in comparative example 3, "modified water-based epoxy resin" is replaced by "water-based epoxy resin". It can be seen from Table 2 that the adhesion, contact angle, corrosion resistance, impact resistance and heat resistance are poorer than those of Example 1, and the corrosion resistance after immersion decreases more. This may be because the water-based epoxy resin has a larger specific surface area and stronger hydrophobicity after being grafted with modified graphene A; in comparative example 4, "modified graphene B" is replaced by "reduced graphene oxide". It can be seen from Table 2 that the adhesion, contact angle, corrosion resistance and heat resistance are better than those of Example 1. The adhesion, contact angle, corrosion resistance, impact resistance and heat resistance of the modified graphene A and modified graphene B are poor, and the corrosion resistance after immersion decreases a lot. This may be because the reduced graphene oxide has better dispersibility after being grafted with 2,6-diaminopyridine, and can also promote the formation of a passivation film on the surface of the metal substrate; Comparative Example 5 replaces "modified graphene A and modified graphene B" with "reduced graphene oxide". It can be seen from Table 2 that compared with Example 1, its adhesion, contact angle, corrosion resistance, impact resistance and heat resistance are poor, and the corrosion resistance after immersion decreases a lot. This may be due to the relatively poor dispersibility and other properties of the reduced graphene oxide; Comparative Example 6 replaces "modified water-based epoxy resin" with "water-based epoxy resin" And "modified graphene B" is replaced by "reduced graphene oxide". It can be seen from Table 2 that compared with Example 1, the adhesion, contact angle, corrosion resistance, immersion resistance, impact resistance and heat resistance are poor, and the corrosion resistance after immersion is greatly reduced. This may be due to the relatively small specific surface area and relatively poor hydrophobicity of the unmodified water-based epoxy resin, and the dispersibility of reduced graphene oxide is relatively poor compared to modified graphene B, and it cannot promote the formation of a passivation film on the surface of the substrate by iron ions; Comparative Example 7 replaces "99.2g of modified water-based epoxy resin" with "99g of water-based epoxy resin" and replaces "0.1g of modified graphene B" with "0.2g of modified graphene A and 0.1g modified graphene B", it can be seen from Table 2 that compared with Example 1, the contact angle, corrosion resistance, immersion resistance, impact resistance and heat resistance are poor, and the corrosion resistance after immersion decreases more. This may be because compared with the modification of water-based epoxy resin with modified graphene A first, adding modified graphene A and modified graphene B at the same time during the production process will greatly reduce the grafting degree of modified graphene A and water-based epoxy resin, making the corrosion resistance, immersion resistance, impact resistance and heat resistance of the final anti-corrosion coating poor.
[0101] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0102] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing an anti-corrosion coating based on modified graphene, characterized in that: The specific steps include: Step S1. Add modified graphene B and dispersant NNO to the modified waterborne epoxy resin in sequence, stir at 75-80° C. and 300-350 r / min for 15-30 min to obtain a premixed coating; Step S2. Add T31 curing agent, tributyl phosphate and leveling agent to the premixed coating, stir at 300-350 r / min for 15-30 min to obtain an anti-corrosion coating based on modified graphene; The modified waterborne epoxy resin is prepared from water, sodium carboxymethyl cellulose, reduced graphene oxide and waterborne epoxy resin; The modified graphene B is prepared from 2,6-diaminopyridine, water and reduced graphene oxide; The reduced graphene oxide is obtained by subjecting graphite oxide to thermal reduction treatment; The preparation method of the reduced graphene oxide is as follows: 20-23 g of graphite oxide is placed in a corundum crucible, and the temperature is gradually raised to 785-800° C. in a nitrogen atmosphere, and kept at 785-800° C. for 10-15 min, and then cooled to 35-50° C. to obtain reduced graphene oxide; The mass ratio of the modified waterborne epoxy resin, the modified graphene B and the dispersant NNO in step S1 is 99.2-101.25:0.1-0.15:1-1.5; The mass ratio of the premixed coating, T31 curing agent, tributyl phosphate and leveling agent in step S2 is 100.3-102.9:4-7:0.1-0.5:0.5-1.
2. The method for preparing the anticorrosive coating based on modified graphene according to claim 1, characterized in that: The leveling agent in step S2 is any one of H633 leveling agent and H850 leveling agent.
3. The method for preparing the anticorrosive coating based on modified graphene according to claim 1, characterized in that: The preparation method of the modified waterborne epoxy resin in step S1 is as follows: Step A1. First, sodium carboxymethyl cellulose was added to water, and stirred at 850-900 r / min for 45-60 min, and then reduced graphene oxide was added, ultrasonicated for 2.5-3 h, purified by ultrafiltration, and then dried in a vacuum at 75-80 ° C for 24-25 h to obtain modified graphene A; Step A2. Add water to the waterborne epoxy resin and stir evenly, then add the modified graphene A and mix, and stir at a speed of 300-350 r / min for 15-20 min to obtain a modified waterborne epoxy resin.
4. The method for preparing the anticorrosive coating based on modified graphene according to claim 3, characterized in that: The mass ratio of water, sodium carboxymethyl cellulose and reduced graphene oxide in step A1 is 83-84: 0.7-1.1:13.5-15; the mass ratio of the waterborne epoxy resin, water and modified graphene A in step A2 is 40-41:59-60:0.2-0.
25.
5. The method for preparing the anticorrosive coating based on modified graphene according to claim 1, characterized in that: The preparation method of the modified graphene B in step S1 is as follows: Step B1. Add reduced graphene oxide into water and perform ultrasonic dispersion treatment for 30-45 min to obtain a graphene dispersion; Step B2. Add 2,6-diaminopyridine to water and stir evenly, then add graphene dispersion, stir at 75-80°C for 30-35 minutes, then dry at 75-80°C, grind, and obtain modified graphene B.
6. The method for preparing the anticorrosive coating based on modified graphene according to claim 5, characterized in that: The mass ratio of water to reduced graphene oxide in step B1 is 90-100:0.2-0.
25.
7. The method for preparing the anticorrosive coating based on modified graphene according to claim 5, characterized in that: The mass ratio of water, 2,6-diaminopyridine and graphene dispersion in step B2 is 18-20: 0.05-0.1:90-100。 8. An anti-corrosion coating based on modified graphene, characterized in that: The anti-corrosion coating is prepared by the preparation method described in any one of claims 1-7.