CO oxidation catalyst as well as preparation method and application thereof
By doping selenium in the titanium dioxide carrier and supporting the precious metal catalyst to form a Ti-O-Se structure, the problem of poisoning and deactivation of the precious metal catalyst in steel flue gas and insufficient resistance to SO2 and HCl is solved, and efficient and stable CO2 is achieved. Oxidation catalytic effect.
Patent Information
- Application Number
- CN202310369067.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Existing precious metal catalysts are easily poisoned and deactivated in steel flue gas, and they lack a CO oxidation catalyst that can resist both SO2 and HCl, making it unable to effectively handle CO emissions in steel flue gas.
Selenium is doped into the titanium dioxide carrier, and the precious metal catalyst is supported on its surface to form a Ti-O-Se and Pt (Ag, Pd, Rh, Ru, Cu)-O-Se structure to improve the catalyst's resistance to SO2 and resistance to HCl performance.
It achieves efficient catalytic CO oxidation at lower temperatures, has high conversion rate and stability, can maintain high-efficiency catalytic performance for a long time in flue gas containing SO2 and HCl, and significantly improves the stability and toxicity resistance of the catalyst.
Smart Images

Figure BDA0004168109720000101 
Figure BDA0004168109720000111 
Figure BDA0004168109720000112
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst and a preparation method and application thereof, and in particular to a CO oxidation catalyst and a preparation method and application thereof. Background Art
[0002] Carbon monoxide (CO) is a colorless, odorless, non-irritating, flammable and toxic gas. Low concentrations of CO in the environment are emitted into the atmosphere, which can cause ozone pollution. Inhalation of CO into the human body can cause cardiovascular diseases, posing a great threat to human living environment and health. CO comes from the incomplete combustion of fossil fuels, and its emission sources include fixed emission sources (such as steel plant waste gas and cement plant waste gas) and mobile emission sources (such as automobile exhaust and ship exhaust). Among CO fixed emission sources, steel plant waste gas accounts for about 30%. Tangshan, Linfen and other regions have issued steel CO emission limit requirements. Therefore, steel CO needs to be urgently controlled.
[0003] The volume fraction of CO in steel flue gas is between 0.5% and 2%, which is suitable for oxidation removal using catalysts. Precious metal catalysts have high CO oxidation activity, and a very small amount of precious metals in the catalyst (<1wt%) can achieve CO removal. However, the application of precious metal catalysts in steel flue gas is limited because steel flue gas (especially sintering flue gas) contains high concentrations of water vapor and SO 2 , HCl and other acidic gases. These acidic gases act in conjunction with water vapor on the precious metal nanoparticles and carriers, causing them to lose the ability to adsorb CO and oxidize CO, resulting in their deactivation.
[0004] In order to solve the problem of poisoning and deactivation of precious metal catalysts, CN111437814A uses tin-doped platinum-titanium catalysts for SO 2 In the CO removal, the tin-doped titanium support can reduce SO 2 adsorption, thereby alleviating the SO 2 CN113751024A prepared a catalyst containing active components and additives by organically combining the impregnation method, precipitation method and ball milling method, which has good CO catalytic performance and sulfur and water resistance. CN200510020701.2 introduced Cl ions into the catalyst in advance to improve the catalyst's performance in CCl 4 Anti-HCl performance in hydrodechlorination reaction. CN201911013707.5 By using the composite oxide heptaaluminate calcium dodecahydrate carrier to load the Pt catalyst, good resistance to Cl poisoning in chlorine-containing organic waste gas was obtained. CN202111653263.9 Using solid acid ZrO 2 The PdCo bimetallic nanoparticles supported on the carrier exhibit high activity and chlorine resistance in chlorine-containing organic waste gas.
[0005] However, in the existing technical solutions, there is no simultaneous SO 2 , HCl CO oxidation precious metal catalyst improvement scheme, while in practical applications, SO 2 The effects of CO and HCl on the catalyst are issues that need to be considered simultaneously. Summary of the invention
[0006] In view of the fact that precious metals are easily poisoned and deactivated during the actual CO removal process, and there is no simultaneous SO 2 The invention provides an improvement scheme for the noble metal catalyst for CO oxidation of HCl. The invention adds selenium to titanium dioxide to form a composite carrier, and loads the noble metal catalyst on the surface of the composite carrier to finally obtain a catalyst with high activity and resistance to SO 2 , HCl-resistant, and highly stable CO catalytic precious metal catalysts.
[0007] According to a first embodiment of the present invention, a CO oxidation catalyst is provided.
[0008] A CO oxidation catalyst comprises a carrier and an active component; the carrier is a titanium dioxide composite carrier doped with selenium; and the active component is a noble metal element.
[0009] Preferably, the noble metal element is selected from one or more of platinum, silver, palladium, rhodium, ruthenium, iridium and copper, preferably platinum.
[0010] Preferably, in the CO oxidation catalyst, the mass fraction of the active component is 0.1 to 1.5%, preferably 0.2 to 1.3%, and more preferably 0.5 to 1%.
[0011] Preferably, in the CO oxidation catalyst, the mass fraction of the selenium element is 0.01-5%, preferably 0.05-3%, more preferably 0.08-1%.
[0012] According to a second embodiment of the present invention, a method for preparing a CO oxidation catalyst is provided.
[0013] A method for preparing a CO oxidation catalyst, the method comprising the following steps:
[0014] 1) dissolving a soluble selenium-containing salt in water to obtain a selenium-containing solution; mixing titanium dioxide with water to obtain a suspension; then adding the selenium-containing solution to the suspension and mixing evenly, and then adding an acid to react. After the reaction is completed, solid-liquid separation is performed to obtain Se@TiO 2 Composite carrier.
[0015] 2) Se@TiO prepared in step 1) 2The composite carrier is mixed with a solution containing noble metal active components, the solid and liquid are separated, and the obtained solid is dried and calcined in sequence to obtain a CO oxidation catalyst.
[0016] Preferably, the soluble selenium-containing salt is one or more of sodium selenosulfate and sodium selenite.
[0017] Preferably, the noble metal active component is one or more of platinum, silver, palladium, rhodium, ruthenium, iridium and copper.
[0018] Preferably, the titanium dioxide is anatase or a mixture of anatase and rutile.
[0019] Preferably, in step 1), the concentration of the selenium-containing solution is 0.5-5 g / L, preferably 1-4 g / L, more preferably 1.5-3.5 g / L; the mixing mass ratio of titanium dioxide to water is 1:3-15, preferably 1:4-12, more preferably 1:5-10.
[0020] Preferably, the acid is a solution of hydrochloric acid and nitric acid, and the pH of the hydrochloric acid solution is 0.1-4, preferably 0.5-3.5, and more preferably 0.8-3.
[0021] Preferably, in step 2), in the solution containing the precious metal active component, the mass concentration of the precious metal active component is 0.5-8 g / L, preferably 1-6 g / L, more preferably 1.5-4 g / L.
[0022] Preferably, Se@TiO 2 The mixing ratio (mass to volume ratio) of the composite carrier to the solution containing the noble metal active component is 1:15-20 g / mL.
[0023] Preferably, step 1) is specifically as follows: adding a soluble selenium-containing salt to deionized water, stirring until completely dissolved (e.g., stirring for 0.5-5 min) to obtain a selenium-containing solution; adding titanium dioxide to deionized water, stirring and mixing evenly (e.g., stirring and mixing for 1-60 min) to obtain a white suspension; mixing the selenium-containing solution and the suspension evenly (e.g., stirring and mixing for 1-30 min), and then slowly dropping a hydrochloric acid solution, performing solid-liquid separation (e.g., suction filtration) after the dropwise addition is completed, and washing the obtained solid with deionized water (e.g., washing 1-5 times) to obtain Se@TiO 2 Composite carrier.
[0024] Preferably, step 2) is specifically: Se@TiO prepared in step 1) 2The composite carrier is added to a solution containing a noble metal active component, and then subjected to ultrasonic treatment and stirring treatment (for example, ultrasonic treatment for 1-60 minutes and then stirring treatment for 1-60 minutes); then the mixed product after the stirring treatment is dried (for example, dried in a drying oven at 100-150° C. for 1-18 hours); after the drying is completed, the dried product is calcined in a muffle furnace at 300-800° C. (preferably 350-600° C.) for 1-12 hours (preferably 2-10 hours); after the calcination is completed, the CO oxidation catalyst is obtained.
[0025] According to a third embodiment of the present invention, a use of a CO oxidation catalyst is provided.
[0026] Application of a CO oxidation catalyst, wherein the CO oxidation catalyst is applied to a water, SO 2 and HCl in the catalytic oxidation removal of CO from flue gas.
[0027] Preferably, the CO oxidation catalyst is applied to water, SO 2 The specific process of removing CO from flue gas by catalytic oxidation is as follows: placing a CO oxidation catalyst into a CO catalytic reaction device, and introducing the flue gas to be treated into the CO catalytic reaction device; CO is adsorbed when passing through the surface of the CO oxidation catalyst and oxidized to CO 2 .
[0028] In the present invention, selenium is doped into a noble metal catalyst with titanium dioxide as a carrier, and a Ti-O-Se and Pt (Ag, Pd, Rh, Ru, Cu)-O-Se structure is formed on the catalyst surface. 2 After the flue gas containing HCl enters the CO catalytic reaction device, CO is adsorbed on the catalyst surface and oxidized to CO 2 , while sulfate and Cl cannot be adsorbed on the catalyst surface, and the CO oxidation catalytic efficiency of the catalyst can reach more than 99%.
[0029] In the present invention, the Ti-O-Se and Pt (Ag, Pd, Rh, Ru, Cu) -O-Se structures on the catalyst surface can effectively reduce the deposition of sulfate on the catalyst surface and the adsorption of Cl on the catalyst surface, and can also strengthen the adsorption of CO on the catalyst surface and enhance the oxidation catalytic effect of CO.
[0030] In the present invention, compared with the prior art, the CO oxidation catalyst provided by the present invention can catalytically oxidize CO at a lower ambient temperature and has a higher conversion rate. 50 (the temperature required for the catalytic efficiency to reach 50%) and T 90Compared with the noble metal catalysts not doped with selenium, the CO catalytic oxidation efficiency of the CO oxidation catalyst provided by the present invention can reach more than 99% when the reaction temperature is above 180°C.
[0031] In the present invention, compared with the prior art, the CO oxidation catalyst provided by the present invention is 2 The catalytic oxidation of CO in flue gas containing selenium and HCl has a conversion rate of more than 90% and does not decay significantly after 50 hours. However, the catalytic oxidation effect of the noble metal catalyst without selenium has a slow decay trend and the CO conversion rate decreases to about 60% after 50 hours.
[0032] In the present invention, the composite carrier is prepared by doping selenium and titanium dioxide. Based on a large number of experiments, the present invention draws the following conclusions: the optimal mass fraction of selenium is 0.1-5%. If it is excessive, the catalytic effect of the precious metal will deteriorate, and if it is insufficient, the precious metal will be degraded in the presence of SO. 2 At the same time, the optimal mass fraction of precious metals is 0.1-1.5%, which can achieve the best CO catalytic oxidation effect. Excessive precious metals may cause the precious metals in the outermost layer of the catalyst to be unable to form a Pt (Ag, Pd, Rh, Ru, Cu)-O-Se structure, and then be poisoned and deactivated, while the precious metals in the inner layer cannot contact with the external gas or the contact surface is small, and the oxidation catalytic effect is poor.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. A CO oxidation catalyst provided by the present invention forms a complex Ti-O-Se and Pt (Ag, Pd, Rh, Ru, Cu)-O-Se structure on the catalyst surface, which can effectively reduce the deposition of sulfate and the adsorption of Cl on the catalyst surface, and at the same time can enhance the adsorption effect of CO on the catalyst surface, and has a good CO catalytic oxidation effect. 2 It has high CO catalytic oxidation efficiency and stability in flue gas containing HCl.
[0035] 2. The CO oxidation catalyst provided by the present invention has a good CO catalytic oxidation effect at a relatively low catalytic temperature, has a relatively low requirement for the flue gas temperature, and can meet the flue gas purification needs in most cases.
[0036] 3. The preparation method of the CO oxidation catalyst provided by the present invention is simple, the raw materials are easily available, and it has good application prospects. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments.
[0038] According to a first embodiment of the present invention, a CO oxidation catalyst is provided.
[0039] A CO oxidation catalyst comprises a carrier and an active component; the carrier is a titanium dioxide composite carrier doped with selenium; and the active component is a noble metal element.
[0040] Preferably, the noble metal element is selected from one or more of platinum, silver, palladium, rhodium, ruthenium, iridium and copper, preferably platinum.
[0041] Preferably, in the CO oxidation catalyst, the mass fraction of the active component is 0.1 to 1.5%, preferably 0.2 to 1.3%, and more preferably 0.5 to 1%.
[0042] Preferably, in the CO oxidation catalyst, the mass fraction of the selenium element is 0.01-5%, preferably 0.05-3%, more preferably 0.08-1%.
[0043] According to a second embodiment of the present invention, a method for preparing a CO oxidation catalyst is provided.
[0044] A method for preparing a CO oxidation catalyst, the method comprising the following steps:
[0045] 1) dissolving a soluble selenium-containing salt in water to obtain a selenium-containing solution; mixing titanium dioxide with water to obtain a suspension; then adding the selenium-containing solution to the suspension and mixing evenly, and then adding an acid to react. After the reaction is completed, solid-liquid separation is performed to obtain Se@TiO 2 Composite carrier.
[0046] 2) Se@TiO prepared in step 1) 2 The composite carrier is mixed with a solution containing noble metal active components, the solid and liquid are separated, and the obtained solid is dried and calcined in sequence to obtain a CO oxidation catalyst.
[0047] Preferably, the soluble selenium-containing salt is one or more of sodium selenosulfate and sodium selenite.
[0048] Preferably, the noble metal active component is one or more of platinum, silver, palladium, rhodium, ruthenium, iridium and copper.
[0049] Preferably, the titanium dioxide is anatase or a mixture of anatase and rutile.
[0050] Preferably, in step 1), the concentration of the selenium-containing solution is 0.5-5 g / L, preferably 1-4 g / L, more preferably 1.5-3.5 g / L; the mixing mass ratio of titanium dioxide to water is 1:3-15, preferably 1:4-12, more preferably 1:5-10.
[0051] Preferably, the acid is hydrochloric acid or nitric acid solution, and the pH of the hydrochloric acid solution is 0.1-4, preferably 0.5-3.5, and more preferably 0.8-3.
[0052] Preferably, in step 2), in the solution containing the precious metal active component, the mass concentration of the precious metal active component is 0.5-8 g / L, preferably 1-6 g / L, more preferably 1.5-4 g / L.
[0053] Preferably, Se@TiO 2 The mixing ratio (mass to volume ratio) of the composite carrier to the solution containing the noble metal active component is 1:15-20 g / mL.
[0054] Preferably, step 1) is specifically as follows: adding a soluble selenium-containing salt to deionized water, stirring until completely dissolved (e.g., stirring for 0.5-5 min) to obtain a selenium-containing solution; adding titanium dioxide to deionized water, stirring and mixing evenly (e.g., stirring and mixing for 1-60 min) to obtain a white suspension; mixing the selenium-containing solution and the suspension evenly (e.g., stirring and mixing for 1-30 min), and then slowly dropping a hydrochloric acid solution, performing solid-liquid separation (e.g., suction filtration) after the dropwise addition is completed, and washing the obtained solid with deionized water (e.g., washing 1-5 times) to obtain Se@TiO 2 Composite carrier.
[0055] Preferably, step 2) is specifically: Se@TiO prepared in step 1) 2 The composite carrier is added to a solution containing a noble metal active component, and then subjected to ultrasonic treatment and stirring treatment (for example, ultrasonic treatment for 1-60 minutes and then stirring treatment for 1-60 minutes); then the mixed product after the stirring treatment is dried (for example, dried in a drying oven at 100-150° C. for 1-18 hours); after the drying is completed, the dried product is roasted in a Marble furnace at 300-800° C. (preferably 350-600° C.) for 1-12 hours (preferably 2-10 hours); after the roasting is completed, the CO oxidation catalyst is obtained.
[0056] According to a third embodiment of the present invention, a use of a CO oxidation catalyst is provided.
[0057] Application of a CO oxidation catalyst, wherein the CO oxidation catalyst is applied to a water, SO 2 and HCl in the catalytic oxidation removal of CO from flue gas.
[0058] Preferably, the CO oxidation catalyst is applied to water, SO 2 The specific process of removing CO from flue gas by catalytic oxidation is as follows: placing a CO oxidation catalyst into a CO catalytic reaction device, and introducing the flue gas to be treated into the CO catalytic reaction device; CO is adsorbed when passing through the surface of the CO oxidation catalyst and oxidized to CO 2 .
[0059] Preparation Example 1
[0060] First, 0.33 g of selenium powder and 0.52 g of sodium sulfite were dissolved in 500 mL of water and stirred to mix evenly. Then, the mixed system was heated to 70° C. and stirred for 4 h to obtain a sodium selenosulfate solution with a concentration of 1.7 g / L, which was stored away from light.
[0061] Example 1
[0062] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0063] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 25 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0064] Example 2
[0065] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0066] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 31 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0067] Example 3
[0068] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0069] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 15 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0070] Example 4
[0071] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0072] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 6 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0073] Example 5
[0074] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0075] 2) Se@TiO prepared in step 1) 2 The composite support was added to 40 mL of 2.8 g / L platinum tetrachloride aqueous solution, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after stirring was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0076] Example 6
[0077] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 6 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0078] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 25 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0079] Example 7
[0080] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 80 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0081] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 25 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0082] Example 8
[0083] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 4 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0084] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 25 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0085] Example 9
[0086] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 240 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0087] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 25 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0088] Example 10
[0089] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0090] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 24 mL of 2.8 g / L palladium chloride, ultrasonically treated for 30 min, and stirred for 30 min. The mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h, and then the obtained dry product was calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0091] Embodiment 11
[0092] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of nitric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0093] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 23 mL of 2.8 g / L silver nitrate, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0094] Comparative Example 1
[0095] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0096] 2) Se@TiO prepared in step 1) 2 The composite support was added to 62 mL of 2.8 g / L platinum tetrachloride aqueous solution, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after stirring was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0097] Comparative Example 2
[0098] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 40 mL of the sodium selenosulfate solution prepared in Preparation Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0099] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 1.5 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0100] Comparative Example 3
[0101] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 450 mL of the sodium selenosulfate solution prepared in Example 1, stir evenly, then dropwise add 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times to obtain Se@TiO 2 Composite carrier.
[0102] 2) Se@TiO prepared in step 1) 2 The composite support was added to an aqueous solution containing 25 mL of 2.8 g / L platinum tetrachloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0103] Comparative Example 4
[0104] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then drop 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times.
[0105] 2) The TiO 2 The carrier was added to an aqueous solution of platinum tetrachloride containing 25 mL of 2.8 g / L, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0106] Comparative Example 5
[0107] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then drop 30 mL of hydrochloric acid with a pH of 1, filter and wash with deionized water three times.
[0108] 2) The TiO 2 The carrier was added to an aqueous solution containing 25 mL of 2.8 g / L palladium chloride, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0109] Comparative Example 6
[0110] 1) Add 5 g of titanium dioxide powder to 30 mL of deionized water, stir for 30 min, then add 30 mL of nitric acid with a pH of 1, filter and wash with deionized water three times.
[0111] 2) The TiO 2 The carrier was added to an aqueous solution containing 23 mL of 2.8 g / L silver nitrate, ultrasonically treated for 30 min, stirred for 30 min, and the mixed product after the stirring treatment was dried in a drying oven at 120° C. for 6 h. The dried product was then calcined at 450° C. for 5 h to obtain a CO oxidation catalyst.
[0112] Comparative Example 7
[0113] Sodium selenate is dissolved in water to form a dissolving solution, wherein the concentration of sodium selenate in water is 0.005 mol / L, and the molar ratio of sodium selenate to titanium oxide is 0.5. The dissolving solution is added to titanium oxide and stirred for 12 hours, polymerized at 90° C. for 10 hours, and then heated to 120° C. for 6 hours. Finally, the polymerized composite sample is calcined in a He atmosphere at a heating rate of 5° C. / min and kept at 700° C. for 5 hours to obtain the composite titanium oxide of the present invention.
[0114] The method of supporting precious metal Pt is based on PtCl 4 It is the precursor of active component, and the concentration is 0.12g Pt / mL of metal precursor solution was used to impregnate the composite titanium oxide in equal volume, and then dried at 30℃ after standing for 4h. 2 The catalyst was prepared by reduction at 300 °C for 2 h under atmosphere.
[0115] The CO oxidation catalysts prepared in Examples 1 to 11 and Comparative Examples 1 to 7 were made into 50-mesh particles, 1.2 mL was taken and placed in a CO catalytic reaction device, and a test flue gas was introduced. The flue gas composition was: 0.5% CO, 16% O 2 、10%H 2 O、N 2 The flow rate of the reaction gas is 1200 mL / min and the space velocity is 60000 h -1 The conversion rate of CO was tested by catalytic oxidation of CO at 140°C, 160°C, 180°C and 200°C. The test results are shown in Table 1.
[0116] The CO oxidation catalysts prepared in Examples 1 to 11 and Comparative Examples 1 to 7 were made into 50-mesh particles, 1.2 mL was taken and placed in a CO catalytic reaction device, and a test flue gas was introduced. The flue gas composition was: 0.5% CO, 16% O 2 、10%H 2 O, 25ppmSO 2 、40ppmHCl、N 2 The flow rate of the reaction gas is 1200 mL / min and the space velocity is 60000 h -1 The temperature was 250°C, and the CO conversion rate was tested just after the flue gas was introduced, and after 24h, 48h, and 64h of the flue gas introduction. The test results are shown in Table 2.
[0117] Table 1
[0118]
[0119]
[0120] Table 2
[0121]
[0122]
[0123] It can be seen from the above experiments that the CO oxidation catalyst provided by the present invention has a high catalytic rate and good anti-poisoning effect. Compared with the existing catalysts, the CO oxidation catalyst provided by the present invention is 50 and T 90 were significantly reduced, and in the presence of SO 2The conversion rate of HCl in flue gas will not decrease significantly for a long time, the service life will be greatly extended, the stability will be greatly improved, and it has good application prospects.
Claims
1. A CO oxidation catalyst, characterized in that: The CO oxidation catalyst comprises a carrier and an active component; the carrier is a titanium dioxide composite carrier doped with selenium; and the active component is a noble metal element.
2. The CO oxidation catalyst according to claim 1, characterized in that: The noble metal element is selected from one or more of platinum, silver, palladium, rhodium, ruthenium, iridium and copper, preferably platinum.
3. The CO oxidation catalyst according to claim 2, characterized in that: In the CO oxidation catalyst, the mass fraction of the active component is 0.1 to 1.5%, preferably 0.2 to 1.3%, more preferably 0.5 to 1%; and / or In the CO oxidation catalyst, the mass fraction of the selenium element is 0.01-5%, preferably 0.05-3%, and more preferably 0.08-1%.
4. A method for preparing a CO oxidation catalyst as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following steps: 1) dissolving a soluble selenium-containing salt in water to obtain a selenium-containing solution; mixing titanium dioxide with water to obtain a suspension; then adding the selenium-containing solution to the suspension and mixing evenly, and then adding an acid to react. After the reaction is completed, solid-liquid separation is performed to obtain a Se@TiO2 composite carrier; 2) The Se@TiO2 composite carrier prepared in step 1) is mixed with a solution containing a noble metal active component, the solid-liquid separation is performed, and the obtained solid is dried and calcined in sequence to obtain a CO oxidation catalyst.
5. The method according to claim 4, characterized in that: The soluble selenium-containing salt is one or more of sodium selenosulfate and sodium selenite; and / or The noble metal active component is one or more of platinum, silver, palladium, rhodium, ruthenium, iridium and copper; and / or The titanium dioxide is anatase or a mixture of anatase and rutile.
6. The method according to claim 4 or 5, characterized in that: In step 1), the concentration of the selenium-containing solution is 0.5-5 g / L, preferably 1-4 g / L, more preferably 1.5-3.5 g / L; the mixing mass ratio of titanium dioxide to water is 1:3-15, preferably 1:4-12, more preferably 1:5-10; and / or The acid is hydrochloric acid or nitric acid solution, and the pH of the acid solution is 0.1-4, preferably 0.5-3.5, and more preferably 0.8-3.
7. The method according to claim 4 or 5, characterized in that: In step 2), the mass concentration of the noble metal active component in the solution containing the noble metal active component is 0.5-8 g / L, preferably 1-6 g / L, more preferably 1.5-4 g / L; and / or The mixing ratio (mass to volume ratio) of the Se@TiO2 composite carrier and the solution containing the precious metal active component is 1:15-20 g / mL.
8. The method according to claim 5 or 6, characterized in that: Step 1) is specifically as follows: adding a soluble selenium-containing salt to deionized water, stirring until completely dissolved (for example, stirring for 0.5-5 minutes) to obtain a selenium-containing solution; adding titanium dioxide to deionized water, stirring and mixing evenly (for example, stirring and mixing for 1-60 minutes) to obtain a white suspension; mixing the selenium-containing solution and the suspension evenly (for example, stirring and mixing for 1-30 minutes), and then slowly dropping a hydrochloric acid solution, performing solid-liquid separation (for example, suction filtration) after the dropping is completed, and washing the obtained solid with deionized water (for example, washing 1-5 times) to obtain a Se@TiO2 composite carrier.
9. The method according to any one of claims 5 to 8, characterized in that: Step 2) is specifically as follows: adding the Se@TiO2 composite carrier prepared in step 1) to a solution containing a precious metal active component, performing an ultrasonic treatment and then stirring the solution (for example, performing an ultrasonic treatment for 1-60 minutes and then stirring the solution for 1-60 minutes); then drying the mixed product after the stirring treatment (for example, drying the mixed product in a drying oven at 100-150°C for 1-18 hours); after drying, calcining the dried product in a muffle furnace at 300-800°C (preferably 350-600°C) for 1-12 hours (preferably 2-10 hours); after calcination, the CO oxidation catalyst is obtained.
10. Use of the CO oxidation catalyst according to any one of claims 1 to 3 or use of the CO oxidation catalyst prepared by the method according to any one of claims 4 to 9, characterized in that: The CO oxidation catalyst is applied to the catalytic oxidation removal of CO from flue gas containing water, SO2 and HCl; Preferably, the application of the CO oxidation catalyst to the catalytic oxidation removal of CO from flue gas containing water, SO2 and HCl is specifically as follows: the CO oxidation catalyst is placed in a CO catalytic reaction device, and the flue gas to be treated is introduced into the CO catalytic reaction device, and CO is adsorbed when passing through the surface of the CO oxidation catalyst and is oxidized to CO2.
Citation Information
Patent Citations
Tin-doped platinum-titanium catalyst as well as preparation method and application thereof
CN111437814A
Composite titanium oxide supported noble metal catalyst for hydrogen peroxide synthesis, and preparation method and application method thereof
CN111871411A
Hydrogenation catalyst and preparation method thereof, and preparation method of N, N-dimethyl cyclohexylamine
CN115814820A
Dehydrogenation catalyst for organic hydrides and method for producing dehydrogenation catalyst for organic hydrides
JP2022034544A
Oxidation catalyst and exhaust gas purification method using same
WO2013132895A1