Preparation method of nano nickel-based composite multilayer film
Through variable frequency power ultrasonic pulse electrodeposition technology and special structural design, the problem of insufficient bonding force and corrosion resistance between the nanocomposite deposition layer and the matrix has been solved, and the preparation of nano-nickel-based multilayer films with high hardness and corrosion resistance has been achieved, significantly improving Improve the corrosion resistance of the film layer.
Patent Information
- Application Number
- CN202410847928.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-15
AI Technical Summary
The lattice spacing between the existing nanocomposite deposition layer and the base metal is large, resulting in weak film-base bonding force and poor corrosion resistance. In particular, research on nano-nickel-based multilayer films with high hardness and high corrosion resistance has been relatively intensive. rare.
Using variable frequency power ultrasonic pulse electrodeposition technology, the film layer is constructed with a special structure, combined with hard nanoparticles and nickel-based multi-layer films, to enhance the film-based bonding force and corrosion resistance. It uses nickel sulfate, water, boric acid, activators and Plating solutions containing components such as graphene oxide are subjected to multi-layer electrodeposition to form a continuous lattice structure to improve corrosion resistance.
It significantly enhances the bonding force and corrosion resistance between the coating and the substrate, improves the hardness and corrosion resistance of the deposited layer, extends the corrosion path, reduces the corrosion rate, and ensures the long-term corrosion resistance of the deposited layer.
Smart Images

Figure CN118773689A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano metal ceramic film preparation and electrochemical deposition, and in particular to a method for preparing a nano nickel-based composite multilayer film. Background Art
[0002] Nanocomposite electrodeposition technology, as a cutting-edge research hotspot in the field of electrodeposition, is centered on introducing nanoparticles into the deposition solution and depositing them together with the matrix metal to form a nanocomposite deposition layer with excellent performance. Compared with traditional electrodeposition methods, the deposition layer prepared by nanocomposite electrodeposition technology not only has outstanding mechanical properties (such as high strength, high hardness and excellent wear resistance), but also has excellent chemical properties (such as corrosion resistance).
[0003] However, current research and practice show that there is often a large lattice spacing between the nanocomposite deposit and the base metal, which leads to weak film-base bonding and unsatisfactory corrosion resistance. With the addition of nanoparticles, although the lattice constant has decreased, how to further improve the bonding strength and corrosion resistance of the nanocomposite deposit and the base is still a difficult problem that needs to be solved in the industry. At present, there are relatively few studies on improving the film-base bonding and long-term corrosion resistance of nanocomposite deposits, especially research on high-hardness, high-corrosion-resistant nano-nickel-based multilayer films is even rarer. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a nano nickel-based composite multilayer film, which adopts a variable frequency power ultrasonic pulse electrodeposition method to construct a special structure film layer to prepare a nano composite multilayer film with high hardness, good corrosion resistance and good film-base bonding strength.
[0005] To achieve the above purpose, the technical solution of the present application is: a method for preparing a nano nickel-based composite multilayer film, comprising:
[0006] Step (1): preparing a basic plating solution according to the main salt formula;
[0007] Step (2): Mix the hard nanoparticles and the surfactant with deionized water, fully suspend and disperse the mixed solution by ultrasonic waves and mechanical stirring of a certain intensity, add the dispersed mixed solution to the basic plating solution prepared in step (1) to obtain a plating solution with added hard nanoparticles, and place the plating solution in an ultrasonic field again for dispersion;
[0008] Step (3): Mix the two nanoparticles with deionized water, fully suspend and disperse the mixed solution by ultrasonic waves of a certain intensity and mechanical stirring, add the dispersed mixed solution to the basic plating solution prepared in step (1) to obtain a plating solution with the two nanoparticles added, and place the plating solution in an ultrasonic field again for dispersion;
[0009] Step (4): adjusting the pH value of the basic plating solution prepared in step (1), the pH value of the plating solution prepared in step (2), and the pH value of the plating solution prepared in step (3) to the process specification;
[0010] Step (5): using a high-purity nickel plate as an anode and an alloy steel matrix workpiece as a cathode, the electrolytic cell is filled with a basic plating solution prepared according to step (1), immersing the nickel plate and the alloy steel matrix workpiece in the basic plating solution, connecting a pulse power supply and an ultrasonic generator between the cathode and the anode for electrodeposition, taking out the nickel plate and the alloy steel matrix workpiece, rinsing them with deionized water, and placing them in the plating solution prepared in step (2), immersing the nickel plate and the alloy steel matrix workpiece in the plating solution, connecting a pulse power supply and an ultrasonic generator between the cathode and the anode for electrodeposition, taking out the nickel plate and the alloy steel matrix workpiece, rinsing them with deionized water, and placing them in the plating solution prepared in step (3), immersing the nickel plate and the alloy steel matrix workpiece in the plating solution, and then connecting a pulse power supply and an ultrasonic generator between the cathode and the anode for electrodeposition.
[0011] In one of the embodiments, before using the alloy steel substrate workpiece as a cathode, it is pretreated, specifically, the substrate surface is mechanically polished with 360#, 600#, 800#, 1000# and 2000# water-abrasive sandpaper, and then cleaned with acetone and ethanol in turn after polishing, and then the substrate is degreased and activated.
[0012] In one embodiment, the electrodeposition process is implemented in a variable frequency power ultrasonic composite deposition system, which includes an ultrasonic generator containing an ultrasonic medium, a support net installed in the ultrasonic generator, a plating tank placed on the support net, and a plating tank containing a plating solution. The plating solution immerses a cathode workpiece and an anode nickel plate connected to a pulse power supply, and the lower part of an electric stirrer extends into the plating solution for stirring.
[0013] In one embodiment, the ratio of the cathode area to the anode area is 1:4-2:3, and the distance between the two electrodes is 23-27 mm.
[0014] In one embodiment, the base plating solution prepared in step (1), the plating solution prepared in step (2), and the plating solution prepared in step (3) include nickel sulfate, water, boric acid, an activator, graphene oxide and hard nanoparticles, one or more inorganic salts, and alkali.
[0015] In one embodiment, the plating solution maintains a graphene oxide concentration of 0.1 g / l to 0.4 g / l; the plating solution maintains a TiN nanoparticle concentration of 0 to 30 g / l.
[0016] In one embodiment, the main salt formula includes the following concentration components: nickel sulfate (NiSO4·6H2O) 250g / l-350g / l, ammonium chloride (NH4Cl) 10g / l-20g / l, boric acid (H3BO3) 20g / l-35g / l, sodium dodecyl sulfate (CH3(CH2) 11 OSO3Na)0.1g / .
[0017] In one embodiment, the electrodeposition process parameters are: forward voltage of 5V to 12V, reverse voltage of 5V to 12V, cathode current density of 1A / dm 2 ~6A / dm 2 , the ultrasonic frequency is 45kHz~80kHz, the ultrasonic power is 150W~300W, the forward pulse duty cycle is 20%~50%, the mechanical stirring speed is 150r / min~400r / min, and the electrodeposition time is 20min~70min when the plating solution temperature is 45℃~50℃.
[0018] In one embodiment, the process conditions for fully suspending and dispersing the mixed solution in steps (2) and (3) are: ultrasonic power 160-190W, action time 18-25min; the process conditions for placing the plating solution in an ultrasonic field again for dispersion are: ultrasonic power 190-220W, action time 8-15min.
[0019] In one embodiment, the pH value is 3.8-4.5.
[0020] The present invention adopts the above technical scheme, and can achieve the following technical effects: the present invention uses alloy steel as the base material, and its face-centered cubic lattice structure matches the face-centered cubic lattice nickel coating prepared by the improved Watt plating solution. When the lattice constants of the two are similar, a continuous lattice structure can be formed, thereby significantly enhancing the bonding force between the coating and the substrate. The present invention uses a pure nickel coating as a base layer, and introduces nanoparticles layer by layer. This multi-layer structure design can effectively extend the corrosion path and reduce the corrosion rate when subjected to corrosion, thereby improving the long-term corrosion resistance of the deposited layer.
[0021] By adopting the method of variable frequency ultrasonic assisted and pulsed electrodeposition, the surface of the deposited nanocomposite electrodeposition layer is smooth, the structure is more dense and uniform, the bonding force between the film layers is strong, and the hardness and corrosion resistance are improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0023] Figure 1 It is a schematic diagram of the structure of the variable frequency power ultrasonic composite deposition system;
[0024] Figure 2 XRD patterns of different types of multilayer films;
[0025] Figure 3 Metallographic diagrams of different types of multilayer films;
[0026] Figure 4 Polarization curves of different types of multilayer films;
[0027] Figure 5 Metallographic images of different types of multilayer films after microbial corrosion;
[0028] Figure 6 Polarization curves of different types of multilayer films after microbial corrosion;
[0029] Explanation of the serial numbers in the figure: 1-anode; 2-cathode; 3-plating solution; 4-pulse power supply; 5-electric stirrer; 6-plating tank; 7-support net; 8-ultrasonic medium; 9-ultrasonic generator. DETAILED DESCRIPTION
[0030] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0031] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0032] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, "multiple" means two or more, unless otherwise clearly and specifically defined. "Several" means one or more, unless otherwise clearly and specifically defined.
[0033] In the description of the present application, it should be understood that the terms "center", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0034] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0035] The present invention adopts a variable frequency power ultrasonic pulse electrodeposition process, adds nano metal ceramic particles into the plating solution, changes the film layer structure and prepares a nickel-based multilayer film. The main salt of the plating solution is nickel sulfate (NiSO4·6H2O), which is mainly used to provide a source of nickel in the composite deposit layer. Ammonium chloride (NH4Cl) and boric acid (H3BO3) are used as main additional salts, wherein ammonium chloride (NH4Cl) acts as an anode activator to help dissolve the anode nickel and increase the conductivity of the plating solution. Boric acid (H3BO3) is used as a buffer to mainly stabilize the pH value of the plating solution and improve the performance of the deposit layer. Sodium dodecyl sulfate (CH3(CH2) 11 OSO3Na) is added as a surfactant mainly to reduce the tension on the electrode surface, thereby making it difficult for hydrogen bubbles to stay on the cathode surface and avoiding pinholes and pitting in the deposition layer. At the same time, it also has a wetting effect on the nanoparticles in the plating solution, which can make the nanoparticles fully wetted and dispersed in the plating solution, thus facilitating the co-deposition of nano-metal ceramic particles and nickel ions.
[0036] In the present invention, the cathode substrate needs to be leveled, and the surface of the substrate material needs to be mechanically leveled to reduce the surface roughness, including grinding, polishing, etc. The leveling process is: the special steel is pre-treated by means of polishing, and the substrate surface is mechanically polished by using 360#, 600#, 800#, 1000# and 2000# water-abrasive sandpapers respectively during the polishing process. During the polishing process, from the perspective of materials science, the surface of the substrate material should be polished from two mutually perpendicular directions and the number of polishing in the two directions should be kept consistent as much as possible. At the same time, the wear marks should be kept small and uniform to ensure the bonding force between the deposited layer and the substrate, while not affecting the flatness of the deposited layer.
[0037] The cathode substrate is treated on the surface to remove possible dust, grease, oxides, etc. The surface treatment process is as follows: first, the surface is cleaned with deionized water, and then the substrate is placed in a degreasing alkali solution at room temperature to clean the grease that may exist on the surface. The degreasing alkali solution consists of: NaOH 80-100g / L, Na3PO450-60g / L, washing powder 3-5g / L, and water as the balance. After alkaline washing, it is rinsed with deionized water and blown dry for use. Then the substrate is acid-washed: CH3(CH2) is prepared 11 OSO3Na 0.02-0.05g / L, 3-5wt.% dilute H2SO4 pickling solution, place the substrate in the pickling solution, can remove the oxide layer on the surface of special steel, and achieve the purpose of surface activation. After pickling, rinse with deionized water, blow dry and place it in the plating tank for electrodeposition process.
[0038] After the cathode substrate is surface treated, a nickel plating layer is electroplated on the substrate surface under constant current conditions. If there are parts that do not need to be electroplated, they can be covered with photoresist, resin or other insulation treatments. Select the cathode and anode materials required for electrodeposition and prepare the plating solution. The plating solution composition is: nickel sulfate (NiSO4·6H2O) 250-350g / l, ammonium chloride (NH4Cl) 10-20g / l, boric acid (H3BO3) 20-35g / l, sodium dodecyl sulfate (CH3(CH2)11OSO3Na) 0.1-0.3g / l, ND nanoparticles 0~25g / l, GO nanoparticles 0-0.45g / l. During the electrodeposition process, the forward voltage is 5V~12V, the reverse voltage is 5V~12V, and the cathode current density is 2A / dm 2 ~6A / dm 2, the ultrasonic frequency is 45kHz~80kHz, the ultrasonic power is 180~300W, the forward pulse duty cycle is 20%~50%, the mechanical stirring speed is 250r / min~400r / min, and the electroplating time is 50min~70min under the condition of the plating solution temperature of 45℃~50℃. The constant current is continuously energized for a period of time. After the electroplating is completed, the power is immediately stopped and the stirring is stopped. Since the plating solution is an acidic environment, the coating needs to be quickly taken out of the plating tank, washed with deionized water, and blown dry. The surface of the nano-composite electrodeposited layer obtained on the substrate by the above-mentioned electroplating method is smoother and flatter, the structure is more uniform, and the hardness and corrosion resistance are significantly improved compared with the substrate and the pure nickel coating.
[0039] Example 1
[0040] This embodiment provides a method for preparing a nano nickel-based composite multilayer film, the specific steps of which are: (1) grinding and polishing the cathode with sandpaper;
[0041] (2) Degreasing with weak alkaline solution;
[0042] (3) Activated with 5% by mass dilute sulfuric acid;
[0043] (4) washing with acetone and ethanol in sequence, washing with deionized water (twice) and air-drying;
[0044] (5) Adjust pH to 4.1;
[0045] (6) placing the workpiece into the plating solution (1) for electrodeposition, and rinsing with deionized water and air-drying after completion;
[0046] (7) placing the workpiece into a plating solution containing the plating solution (2) for electrodeposition, and rinsing with deionized water and air-drying after completion;
[0047] (8) placing the workpiece into the plating solution (3) for electrodeposition, and after the electrodeposition, taking out the workpiece, rinsing it with deionized water and air-drying it to obtain a Ni / Ni-ND / Ni-ND-GO nickel-based composite multilayer film;
[0048] The composition and process conditions of the plating solution (1) in step (6) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L. During the electrodeposition process, the cathode current density was 4A / dm 2 , the ultrasonic frequency is 45kHz:80kHz=20s:10s, the ultrasonic power is 300W, the plating solution temperature is 50°C, and the electrodeposition time is 60min.
[0049] The composition and process conditions of the plating solution (2) in step (7) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L, ND nanoparticles 15g / L. During the electrodeposition process, the cathode current density was 3A / dm 2 , the ultrasonic frequency is 45kHz:80kHz=10s:20s, the ultrasonic power is 150W, the plating solution temperature is 50℃, and the electrodeposition time is 60min.
[0050] The composition and process conditions of the plating solution (1) in step (8) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L, ND nanoparticles 15g / L, GO nanoparticles 0.25g / L. During the electrodeposition process, the cathode current density was 4A / dm 2 , the ultrasonic frequency is 45kHz:80kHz=20s:10s, the ultrasonic power is 300W, the plating solution temperature is 50°C, and the electrodeposition time is 60min.
[0051] The surface of the Ni / Ni-ND / Ni-ND-GO nickel-based composite multilayer film prepared in this example is smooth and has high density. The electrochemical corrosion resistance test shows that the corrosion potential of the composite deposition layer is -0.673V and the self-corrosion current is 1.96x10 -7 A. The corrosion potential of the composite deposit layer is positively shifted compared with the substrate, and the corrosion current of the composite deposit layer is 2 orders of magnitude smaller than that of the substrate, indicating that the composite deposit layer has the lowest corrosion rate and the best corrosion resistance. The corrosion resistance of the substrate material is significantly improved. The microbial corrosion resistance test shows that there is no obvious corrosion on the surface of the coating after corrosion, and the corrosion current density decreases by one order of magnitude. The lattice constant of the substrate is a=7.3311, the lattice constant of the Ni deposit layer is a=6.5594, the lattice constant of the Ni / Ni-ND double-layer deposit layer is a=5.1904, and the lattice constant of the Ni / Ni-ND / Ni-ND-GO multilayer deposit layer is a=3.5372. This is because the lattice constant of the deposit layer gradually decreases with the addition of nanoparticles, and the stress generated by the coordination of the substrate and the deposit layer is released.
[0052] Example 2
[0053] This embodiment provides a method for preparing a nano nickel-based composite multilayer film, the specific steps of which are: (1) grinding and polishing the cathode with sandpaper;
[0054] (2) Degreasing with weak alkaline solution;
[0055] (3) Activated with 5% by mass dilute sulfuric acid;
[0056] (4) washing with acetone and ethanol in sequence, washing with deionized water (twice) and air-drying;
[0057] (5) Adjust pH to 4.1;
[0058] (6) Place the workpiece in the plating solution (1) for electrodeposition, rinse with deionized water and air dry.
[0059] (7) placing the workpiece into a plating solution containing the plating solution (2) for electrodeposition, and rinsing with deionized water and air-drying after completion;
[0060] (8) placing the workpiece into the plating solution (3) for electrodeposition, and after the electrodeposition, taking out the workpiece, rinsing it with deionized water and air-drying it to obtain a Ni / Ni-TiN / Ni-TiN-GO nickel-based composite multilayer film;
[0061] The composition and process conditions of the plating solution (1) in step (6) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L. During the electrodeposition process, the cathode current density was 4A / dm 2 , the ultrasonic frequency is 45kHz:80kHz=20s:10s, the ultrasonic power is 300W, the plating solution temperature is 50℃, and the electrodeposition time is 50min.
[0062] The composition and process conditions of the plating solution (2) in step (7) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L, TiN nanoparticles 15g / L. During the electrodeposition process, the cathode current density was 4A / dm 2 , the ultrasonic frequency is 45kHz:80kHz=10s:20s, the ultrasonic power is 150W, the plating solution temperature is 50℃, and the electrodeposition time is 50min.
[0063] The composition and process conditions of the plating solution (1) in step (8) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L, TiN nanoparticles 15g / L, GO nanoparticles 0.3g / L. During the electrodeposition process, the cathode current density was 4A / dm 2, the ultrasonic frequency is 45kHz:80kHz=20s:10s, the ultrasonic power is 300W, the plating solution temperature is 50℃, and the electrodeposition time is 50min.
[0064] The surface of the Ni / Ni-TiN / Ni-TiN-GO nickel-based composite multilayer film prepared in this example is smooth and has high density. The electrochemical corrosion resistance test shows that the corrosion potential of the composite deposition layer is -0.673V and the self-corrosion current is 2.714x10 -7 A. The corrosion resistance of the substrate material is significantly improved. The microbial corrosion resistance test shows that no obvious corrosion occurs on the surface of the coating after corrosion, and the corrosion current density decreases by one order of magnitude. The lattice constant of the substrate is a=7.3311, the lattice constant of the Ni deposition layer is a=6.987, the lattice constant of the Ni / Ni-TiN double-layer deposition layer is a=5.522, and the lattice constant of the Ni / Ni-TiN / Ni-TiN-GO multilayer deposition layer is a=3.258. This is because the lattice constant of the deposition layer gradually decreases with the addition of nanoparticles, and the stress generated by the coordination between the substrate and the deposition layer is released.
[0065] Comparative Example 1
[0066] A method for preparing a nano nickel-based composite multilayer film is provided, the specific steps of which are:
[0067] (1) Cathode sandpaper grinding and polishing;
[0068] (2) Degreasing with weak alkaline solution;
[0069] (3) Activated with 5% by mass dilute sulfuric acid;
[0070] (4) washing with acetone and ethanol in sequence, washing with deionized water (twice) and air-drying;
[0071] (5) Adjust pH to 4.1;
[0072] (6) variable frequency power ultrasonic electrodeposition of a nickel-based composite deposition layer in a plating solution containing nanoparticles, and then taking it out and rinsing it with deionized water;
[0073] (7) Repeat step (6) (twice);
[0074] (8) Blow dry;
[0075] The composition and process conditions of the composite plating solution in step (6) of the above method are: NiSO4·6H2O 300 g / l, NH4Cl 15 g / l, H3BO 30 g / l, CH3 (CH2) 11 OSO3Na 0.02g / L, ND nanoparticles 15g / L, GO nanoparticles 0.25g / L. During the electrodeposition process, the cathode current density was 4A / dm2 , the ultrasonic frequency is 45kHz:80kHz=20s:10s, the ultrasonic power is 180W, the pulse duty cycle is 30%, and the electrodeposition time is 60min under the condition of the plating solution temperature of 50°C.
[0076] The corrosion current density of the Ni-ND-GO composite multilayer film prepared in this comparative example is 5.69×10 -5 A.cm -2 After microbial corrosion, obvious corrosion occurred on the coating surface, and the corrosion current density decreased by an order of magnitude. The XRD diagram showed that the (111) crystal plane was significantly shifted.
[0077] Comparative Example 2
[0078] A method for preparing a nano nickel-based composite multilayer film is provided, the specific steps of which are:
[0079] (1) Cathode sandpaper grinding and polishing;
[0080] (2) Degreasing with weak alkaline solution;
[0081] (3) Activated with 5% by mass dilute sulfuric acid;
[0082] (4) washing with acetone and ethanol in sequence, washing with deionized water (twice) and air-drying;
[0083] (5) Adjust pH to 4.1;
[0084] (6) variable frequency power ultrasonic electrodeposition of a nickel-based composite deposition layer in a plating solution containing nanoparticles, and then taking it out and rinsing it with deionized water;
[0085] (7) Repeat step (6) (twice);
[0086] (8) Blow dry;
[0087] The composition and process conditions of the composite plating solution in step (6) of the above method are: NiSO4·6H2O 300g / l, NH4Cl15g / l, H3BO330g / l, CH3(CH2) 11 OSO3Na0.02g / L, TiN nanoparticles 15g / L, GO nanoparticles 0.25g / L. During the electrodeposition process, the cathode current density was 4A / dm 2 , the ultrasonic frequency is 45kHz:80kHz=20s:10s, the ultrasonic power is 180W, the pulse duty cycle is 30%, and the electrodeposition time is 60min under the condition of the plating solution temperature of 50°C.
[0088] The corrosion current density of the Ni-TiN-GO composite multilayer film prepared in this comparative example is 8.96×10 -5 A.cm-2 After microbial corrosion, obvious corrosion occurs on the surface of the coating, and the corrosion current density decreases by an order of magnitude. The XRD diagram shows that the (111) crystal plane has an obvious shift.
[0089] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.
Claims
1. A method for preparing a nano nickel-based composite multilayer film, characterized in that: include: Step (1): preparing a basic plating solution according to the main salt formula; Step (2): Mix the hard nanoparticles and the surfactant with deionized water, fully suspend and disperse the mixed solution by ultrasonic and mechanical stirring, add the dispersed mixed solution to the basic plating solution prepared in step (1) to obtain a plating solution with added hard nanoparticles, and place the plating solution in an ultrasonic field again for dispersion; Step (3): Mix the two nanoparticles with deionized water, fully suspend and disperse the mixed solution by ultrasonic and mechanical stirring, add the dispersed mixed solution to the basic plating solution prepared in step (1) to obtain a plating solution with the two nanoparticles added, and place the plating solution in an ultrasonic field again for dispersion; Step (4): adjusting the pH value of the basic plating solution prepared in step (1), the pH value of the plating solution prepared in step (2), and the pH value of the plating solution prepared in step (3) to the process specification; Step (5): A nickel plate with a purity of 99% is used as an anode and an alloy steel matrix workpiece is used as a cathode. The electrolytic cell is filled with a basic plating solution prepared according to step (1). The nickel plate and the alloy steel matrix workpiece are immersed in the basic plating solution. A pulse power supply and an ultrasonic generator are connected between the cathode and the anode for electrodeposition. The nickel plate and the alloy steel matrix workpiece are taken out, rinsed with deionized water, and placed in the plating solution prepared in step (2). The nickel plate and the alloy steel matrix workpiece are immersed in the plating solution. A pulse power supply and an ultrasonic generator are connected between the cathode and the anode for electrodeposition. The nickel plate and the alloy steel matrix workpiece are taken out, rinsed with deionized water, and placed in the plating solution prepared in step (3). The nickel plate and the alloy steel matrix workpiece are immersed in the plating solution. A pulse power supply and an ultrasonic generator are connected between the cathode and the anode for electrodeposition.
2. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: Before using the alloy steel substrate workpiece as the cathode, it was pretreated, specifically, the substrate surface was mechanically polished with 360#, 600#, 800#, 1000# and 2000# water-abrasive sandpaper, and then cleaned with acetone and ethanol in turn after polishing, and then the substrate was degreased and activated.
3. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: The electrodeposition process is implemented in a variable frequency power ultrasonic composite deposition system, which includes an ultrasonic generator containing an ultrasonic medium, a support net installed inside the ultrasonic generator, a plating tank placed on the support net, and a plating solution in the plating tank. The plating solution immerses the cathode workpiece and the anode nickel plate connected to the pulse power supply, and the lower part of the electric stirrer extends into the plating solution for stirring.
4. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: The ratio of the cathode area to the anode area is 1:4-2:3, and the distance between the two electrodes is 23-27 mm.
5. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: The basic plating solution prepared in step (1), the plating solution prepared in step (2), and the plating solution prepared in step (3) comprise nickel sulfate, water, boric acid, an activator, graphene oxide, and one or more inorganic salts of hard nanoparticles, and an alkali.
6. The method for preparing a nano nickel-based composite multilayer film according to claim 5, characterized in that: The plating solution maintains a graphene oxide concentration of 0.1 g / l to 0.4 g / l; the plating solution maintains a TiN nanoparticle concentration of 0 to 30 g / l.
7. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: The main salt formula includes the following concentration components: nickel sulfate (NiSO4·6H2O) 250g / l-350g / l, ammonium chloride (NH4Cl) 10g / l-20g / l, boric acid (H3BO3) 20g / l-35g / l, sodium dodecyl sulfate (CH3(CH2)11OSO3Na) 0.1-0.3g / l.
8. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: The electrodeposition process parameters are: forward voltage of 5V to 12V, reverse voltage of 5V to 12V, cathode current density of 1A / dm 2 ~6A / dm 2 , the ultrasonic frequency is 45kHz~80kHz, the ultrasonic power is 150W~300W, the forward pulse duty cycle is 20%~50%, the mechanical stirring speed is 150r / min~400r / min, and the electrodeposition time is 20min~70min when the plating solution temperature is 45℃~50℃.
9. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: In steps (2) and (3), the process conditions for fully suspending and dispersing the mixed solution are: ultrasonic power 160-190W, action time 18-25min; the process conditions for placing the plating solution in an ultrasonic field again for dispersion are: ultrasonic power 190-220W, action time 8-15min.
10. The method for preparing a nano nickel-based composite multilayer film according to claim 1, characterized in that: The pH value is 3.8-4.5.
Citation Information
Cited By
High-corrosion-resistance amorphous alloy electroplating method
CN122235795A