Process method for gradually changing and dyeing surface of anode product

Through the use of degreasing, neutralizing, chemical polishing and centrifugal drying devices, the problem of difficulty in removing moisture with traditional drying methods is solved, uniform and lasting dyeing and drying of the anode product surface is achieved, and production efficiency and product quality are improved.

CN118773697APending Publication Date: 2024-10-15RI SHAN COMPUTER ACCESSORY (JIASHAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036728.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-10-15

AI Technical Summary

Technical Problem

Traditional oven drying or air drying methods are difficult to completely remove the moisture in the inner cavity gaps and surface residual moisture of aluminum alloy anodized products, resulting in damage to the anodized film and undesirable phenomena such as discoloration, white spots, and watermarks.

Method used

After degreasing, neutralizing, and chemical polishing, the water is quickly removed through the steps of oxidation, background dyeing, ultrapure water rinsing, rapid drying, gradient dyeing, hole sealing, and drying, combined with a centrifugal drying device to ensure that the surface is Dry thoroughly.

Benefits of technology

It improves the dyeing effect and stability, avoids the occurrence of abnormal colors, white spots, and watermarks, enhances the adhesion and durability of dyes, improves production efficiency and product consistency, and meets environmental friendliness and safety requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118773697A_ABST
    Figure CN118773697A_ABST
Patent Text Reader

Abstract

The invention provides a process method for gradient dyeing of the surface of an anode product. The process method comprises the following steps: S1, pretreatment: sequentially including hanging, degreasing, neutralizing and chemical polishing; s2, oxidation; s3, bottom color dyeing; s4, rinsing is carried out; s5, quick water drying: putting the rinsed anode product and a hanger into a centrifugal spin-drying device together, and starting the spin-drying device to rotate at a high speed, so that residual water on the surface of the anode product is quickly spin-dried in the rotating process; s6, gradient color dyeing is conducted, specifically, the hanging tool loaded with the anode product is put into gradient color dyeing liquid to be soaked, and dye components of the gradient color dyeing liquid are metal composite toner and dextrin; s7, hole sealing; and S8, drying. The centrifugal spin-drying device is used for rapidly drying water, water and liquid left on the surface of the anode product are effectively removed, and the defects of different colors, white points, watermarks and the like are avoided. According to the method, the time is saved, the production efficiency and the product consistency are improved, and the yield is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of anodizing, and relates to a gradient dyeing, in particular to a process method for gradient dyeing of the surface of an anode product. Background Art

[0002] Anodic dyeing of aluminum alloy is a common surface treatment technology, which can improve the corrosion resistance and aesthetics of aluminum alloy. Anodizing is a process of forming an oxide layer on the surface of aluminum alloy by electrochemical methods. This process is carried out by immersing the aluminum part as the anode (positive electrode) in an electrolyte solution under a certain voltage. This treatment can form a strong and dense oxide layer, which improves the corrosion resistance and wear resistance of the aluminum alloy. Anodic dyeing is the process of immersing the aluminum alloy in a dye solution after anodizing it so that it absorbs the dye color. The advantages of anodizing dyeing are: 1. Aesthetics: Anodic dyeing allows the surface of aluminum alloy to present a variety of colors, increasing its design flexibility and aesthetics. 2. Corrosion resistance: The oxide layer formed by anodizing itself has good corrosion resistance, and anodizing dyeing can further improve its surface corrosion resistance. 3. Hardness: The surface after anodizing is usually harder than the original aluminum alloy, which improves its wear resistance and scratch resistance.

[0003] With the development of science and technology and the increasing demand of consumers for the appearance of electronic equipment, the two-color gradient color on the surface of aluminum alloy is widely used in the product appearance design in various fields such as home appliances, 3C, and communications due to its unique visual effects and appeal. The reasonable use of two-color gradient color matching can attract the user's visual focus, enhance the beauty of the product, enrich the visual senses, and can adapt to different product design needs.

[0004] For example, Chinese patent document 202210018700.8 discloses a gradient color anodizing equipment and its process, including a special gradient color dyeing machine and a dyeing tank equipped with a special formula potion, including the following steps: step S1: sandblasting the surface, and hanging the outer surface of the material after sandblasting; step S2: alkalinization and cleaning in sequence through the special dyeing formula in the dyeing tank; step S3: cleaning twice after neutralization, chemical polishing after cleaning, and cleaning again twice after cleaning, anodizing after cleaning, continue cleaning twice, ultrasonic cleaning 3 times and hot water cleaning; step S4: drying after cleaning, gradient color treatment after drying, so that the outer surface has a coloring layer and then uses a sealing agent solution to seal the holes; step S5: continue cleaning twice and drying, and finally hang, fully inspect and package. The process conditions of the present invention are simple, easy to implement, can save resources, reduce production costs, and shorten the production cycle.

[0005] In the above technical solution, during the production process of gradient products, the products are dried before dyeing due to the need for gradient effect. However, for products with complex structures, traditional oven drying or air drying methods are not only difficult to completely remove moisture in the inner cavity gaps, but also unable to effectively remove residual moisture on the surface of the product. This will not only damage the anodized film on the surface of the product, but also cause the surface of the product to absorb a large amount of air dust and small particles of foreign matter, resulting in defects such as discoloration, white spots, and watermarks. Summary of the invention

[0006] The purpose of the present invention is to solve the above problems in the prior art and to propose a process for gradual dyeing of the surface of an anode product.

[0007] The object of the present invention can be achieved by the following technical scheme: A process for gradually dyeing the surface of an anode product, characterized in that it comprises the following steps:

[0008] S1. Pre-treatment: including hanging, degreasing, neutralization and chemical polishing;

[0009] S2. Oxidation: Place the hanger containing the anode product into the oxidation solution, so that the anode product is completely immersed in the oxidation solution for oxidation treatment;

[0010] S3, dyeing the base color: soaking the hanger with the anode product in the base color dye solution, the dye components of the base color dye solution are metal composite color powder and dextrin;

[0011] S4, rinsing: After the anode product has been dyed to reach a predetermined color difference value L, the anode product is subjected to multiple ultrapure water rinsing processes;

[0012] S5, quick drying: put the rinsed anode product and the hanger into the centrifugal drying device, start the drying device to rotate at high speed, so that the residual water on the surface of the anode product is quickly dried during the rotation process;

[0013] S6, dyeing with gradient color: soaking the hanger with the anode product in the gradient color dyeing solution, the dye components of the gradient color dyeing solution are metal composite color powder and dextrin;

[0014] S7, sealing: placing the hanger with the anode product into the sealing solution, so that the anode product is completely immersed in the sealing solution for sealing treatment;

[0015] S8, drying: drying the anode product.

[0016] Preferably, in the degreasing in step S1: the hanger containing the anode product is placed in the degreasing solution, and the anode product is completely immersed in the degreasing solution for degreasing treatment; the solution composition of the degreasing solution is 5% sodium silicate, 10% chelating agent, 15% surfactant, 65% water, and 5% corrosion inhibitor; the solution concentration of the degreasing solution is 60±5g / L, the solution temperature is 60±2°C, and the immersion time of the anode product is 180±30s.

[0017] Preferably, in the neutralization in step S1, the hanger containing the anode product is placed in the neutralization solution, and the anode product is completely immersed in the neutralization solution for neutralization treatment; the neutralization solution is nitric acid, the solution concentration of the neutralization solution is 300-400g / L, and the immersion time of the anode product is 120±60S.

[0018] Preferably, in step S1, the chemical polishing includes placing a hanger containing the anode product into a chemical polishing solution, so that the anode product is completely immersed in the chemical polishing solution for chemical polishing; the chemical polishing solution is a mixture of nitric acid and phosphoric acid, the solution concentration of H3PO4 in the chemical polishing solution is 1200±100g / L, the solution concentration of H2SO4 is 240±30g / L, the specific gravity of the chemical polishing solution is 1.770-1.85, and the concentration of aluminum ions produced by the chemical polishing solution for chemical polishing of aluminum products is 10-30g / L.

[0019] Preferably, in step S2, the oxidizing solution is sulfuric acid, and the solution components of the oxidizing solution include H2S04 concentration of 200±10g / L and Al3+ concentration of 0.5-15g / L; the temperature of the oxidizing solution is 19±1°C; the power-on voltage of the oxidizing solution is 15.0±0.5V; and the immersion time of the anode product is 2600±500s.

[0020] Preferably, in step S3, the dye components of the base color dye solution include 30% metal composite color powder, 68.5% dextrin, and a sustained-release agent; the metal composite color powder includes two dyes, one dye has a concentration of 0.4-0.6 g / L, and the other dye has a concentration of 0.01-0.02 g / L; the dextrin is 5-chloro-2-methyl-3-ketone with a proportion of 1.5%; the sustained-release agent is Na2SO4 with a concentration of 1 g / L; the pH value of the base color dye solution is 5-6.

[0021] Preferably, in step S4, the color difference value L / a / b is predetermined, wherein L is 78 to 79.8; a is -106 to -11.1; b is -21.06 to -22.06; and the number of ultrapure water rinsing is 3 times.

[0022] Preferably, in step S5, the centrifugal drying device comprises a drying drum and a centrifugal motor, the centrifugal motor is connected to the drying drum, the centrifugal motor comprises a rotor, a stator, a housing and an end cover, the rotor is disc-shaped, a support bearing is arranged at the center of the rotor, the rotor rotates relative to the stator, and the stator has a cylindrical housing;

[0023] In step S5, the specific steps of quickly drying water include:

[0024] a. Preparation stage: Check whether the centrifugal drying device is intact and ensure that it can operate normally; prepare the work area and ensure that it is clean and tidy to avoid contamination of the product;

[0025] b. Loading products: Load the products onto the fixture and ensure that the products are fixed and stable and will not fall off or shift during the drying process;

[0026] c. Drying operation: put the hanger and the products on it into the spin-drying drum, and make sure that the hanger is firmly connected to the platform of the spin-drying drum; start the centrifugal motor to drive the spin-drying drum to rotate around the center line;

[0027] Preferably, in step S6, the dye components of the gradient dye solution include 30% metal composite color powder, 68.5% dextrin, and a sustained-release agent; the metal composite color powder includes two dyes, one dye has a concentration of 2.5-3.5 g / L, and the other dye has a concentration of 0.8-1.2 g / L; the dextrin is 5-chloro-2-methyl-3-ketone at a ratio of 1.5%; the sustained-release agent is Na2SO4 at a concentration of 1 g / L; the pH value of the base color dye solution is 5-7.

[0028] Preferably, in step S7, the sealing solution comprises 75% nickel acetate, 5% sodium acetate and 20% chelating agent; the temperature of the sealing solution is 95±3°C; the immersion time of the anode product is 2400S; the concentration of the sealing solution is 10-12g / L; and the pH value of the sealing solution is 5.5-6.0.

[0029] Compared with the prior art, the process method for gradual dyeing of the surface of anode products has the following beneficial effects:

[0030] 1. Improve dyeing effect and stability: Through degreasing, neutralization, chemical polishing and other steps, the grease, oxides and other impurities on the surface of the anode product are effectively removed, creating a good surface treatment foundation for the subsequent dyeing process. These steps not only make the dyeing effect more uniform and lasting, but also ensure that the gradient dye fully penetrates into the surface microporous structure of the anode product, enhancing the stability and durability of the dyeing.

[0031] 2. Optimize the base color dyeing liquid formula: The ratio of metal composite color powder and dextrin in the base color dyeing liquid is precisely adjusted to ensure the uniformity and adaptability of the base color. The addition of dextrin not only helps the adhesion and stability of the dye, but also adjusts the viscosity and fluidity of the dyeing liquid, improving the consistency and appearance quality of the dyeing.

[0032] 3. Precise control of the dyeing process: In the steps of dyeing the base color and gradient color, the predetermined color difference value L and the composition of the gradient dye solution are strictly controlled to ensure that the anode product achieves the color change effect required by the design. The multiple applications of the ultrapure water rinsing process further ensure the fixation of the dye and the accuracy of the color.

[0033] 4. Efficient water removal: Use centrifugal drying device to quickly dry water, effectively remove residual water and liquid on the surface of anode products, and avoid the generation of defects such as discoloration, white spots, watermarks, etc. This method not only saves time, but also improves production efficiency and product consistency, and improves yield.

[0034] 5. Environmental friendliness and safety: The solution composition and process steps used are designed with environmental protection and operational safety in mind, avoiding environmental pollution and operator safety risks, and meeting the requirements of modern manufacturing for environmental protection and health and safety.

[0035] In summary, the process method of the invention can not only effectively realize the gradient dyeing of the surface of the anode product, but also show significant advantages in dyeing effect, stability, production efficiency and environmental safety. At the same time, it optimizes the drying method and achieves a fast and thorough drying effect through centrifugal force. It is suitable for application scenarios with large-scale production and high quality requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Flow chart of this process method.

[0037] Figure 2 This is the gradient dyeing ratio diagram of this process method.

[0038] Figure 3 Schematic diagram of the gradient dyeing process of this process method.

[0039] Figure 4 This is the finished product picture of this process method. DETAILED DESCRIPTION

[0040] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.

[0041] like Figure 1 As shown, the process for gradually dyeing the surface of the anode product comprises the following steps:

[0042] S1. Hanging: Hang the anode products on the hanger so that each anode product is on a horizontal plane;

[0043] S2, degreasing: put the hanger with the anode product into the degreasing solution, so that the anode product is completely immersed in the degreasing solution for degreasing treatment;

[0044] In step S2, the degreasing solution comprises 5% sodium silicate, 10% chelating agent, 15% surfactant, 65% water and 5% corrosion inhibitor; the concentration of the degreasing solution is 60±5g / L, the solution temperature is 60±2°C, and the immersion time of the anode product is 180±30s.

[0045] S3, neutralization: placing the hanger containing the anode product into the neutralization solution, so that the anode product is completely immersed in the neutralization solution for neutralization treatment;

[0046] In step S3, the neutralizing solution is nitric acid, the concentration of the neutralizing solution is 300-400 g / L, and the optimal concentration is 350 g / L; the immersion time of the anode product is 120±60S.

[0047] S4, chemical polishing: put the hanger containing the anode product into the chemical polishing solution, so that the anode product is completely immersed in the chemical polishing solution for chemical polishing treatment;

[0048] In step S4, the chemical polishing solution is a mixture of nitric acid and phosphoric acid, specifically using 85% H3PO4 and 98% H2S04, and mixing them in a ratio of H3PO4:H2S04 of 1:5-5.5 to prepare the chemical polishing solution. The concentration of H3PO4 in the chemical polishing solution is 1200±100g / L, the concentration of H2S04 is 240±30g / L, the specific gravity of the chemical polishing solution is 1.770-1.85, and the optimal specific gravity is 1.8; the concentration of aluminum ions produced by the chemical polishing solution for the aluminum product is 10-30g / L.

[0049] S5. Oxidation: Place the hanger containing the anode product into the oxidation solution, so that the anode product is completely immersed in the oxidation solution for oxidation treatment;

[0050] In step S5, the oxidizing solution is sulfuric acid, and the solution components of the oxidizing solution include H2S04 concentration of 200±10g / L, Al3+ concentration of 0.5-15g / L, and the optimal concentration of 8g / L; the temperature of the oxidizing solution is 19±1°C; the power-on voltage of the oxidizing solution is 15.0±0.5V; and the immersion time of the anode product is 2600±500s.

[0051] S6, dyeing the base color: soaking the hanger with the anode product in the base color dye solution, the dye components of the base color dye solution are metal composite color powder and dextrin;

[0052] In step S6, the dye components of the base color dye solution include 30% metal composite color powder, 68.5% dextrin, and a sustained-release agent; the metal composite color powder includes two dyes, one dye (Ono 507) has a concentration of 0.4-0.6g / L, and the optimal concentration is 0.5g / L, and the concentration of the other dye (Ono 502) is 0.01-0.02g / L, and the optimal concentration is 0.015g / L; dextrin is 5-chloro-2-methyl-3-ketone with a proportion of 1.5%; the sustained-release agent is Na2SO4 with a concentration of 1g / L; the pH value of the base color dye solution is 5-6.

[0053] S7, rinsing: after the anode product has been dyed to reach a predetermined color difference value L, the anode product is subjected to multiple ultrapure water rinsing processes;

[0054] In step S7, the color difference value L / a / b is predetermined, wherein L is 78 to 79.8; a is -106 to -11.1; b is -21.06 to -22.06; and the number of ultrapure water rinses is 3 times.

[0055] L / a / b is the color difference value, L represents depth, the higher the value, the lighter the color, the lower the value, the darker the color; a represents red and green, the larger the a value, the redder the color, the smaller the a value, the greener the color; b represents yellow and blue, the larger the a value, the yellower the color, the smaller the a value, the bluer the color.

[0056] S8. Quick drying: Put the rinsed anode product together with the hanger into the centrifugal drying device, start the drying device to rotate at high speed, so that the residual water on the surface of the anode product can be quickly dried during the rotation process, so as to achieve the purpose of quick drying.

[0057] In step S8, the centrifugal drying device includes a drying drum and a centrifugal motor, the centrifugal motor is connected to the drying drum, the centrifugal motor includes a rotor, a stator, a housing and an end cover, the rotor is disc-shaped, a support bearing is arranged at the center of the rotor, the rotor and the stator rotate relative to each other, and the stator has a cylindrical housing;

[0058] The centrifugal motor uses centrifugal force to generate torque. When its rotor rotates, it can drive the centrifugal block to move centrifugally, generate centrifugal force output, and thus achieve the purpose of centrifugal drive. By adding the centrifugal drying process, the residual moisture on the surface can be quickly removed, and the moisture can be removed thoroughly, avoiding the occurrence of defects such as discoloration, white spots, and watermarks.

[0059] In step S8, the specific steps of quickly drying water include:

[0060] a. Preparation stage: Check whether the centrifugal drying device is intact and ensure that it can operate normally; prepare the work area and ensure that it is clean and tidy to avoid contamination of the product;

[0061] b. Loading products: Load the products onto the fixture and ensure that the products are fixed and stable and will not fall off or shift during the drying process;

[0062] c. Drying operation: put the hanger and the product on it into the spin-drying drum, and ensure that the hanger is firmly connected to the platform of the spin-drying drum; start the centrifugal motor to drive the spin-drying drum to rotate around the center line; in actual application, rotate the aluminum product in a clockwise direction at a speed of 300 for 5 minutes, and visually check that there is no moisture residue on the surface of the product.

[0063] During the drying process, the residual liquid on the surface of the product is thrown out under the action of centrifugal force, thereby achieving the purpose of removing residual water and liquid. The drying process of gradient anode products is an important link to ensure product quality and the stability of gradient effect. By following the above reasonable process flow, the residual water on the surface of the workpiece can be effectively removed, the cleanliness of the workpiece surface and the integrity of the gradient effect can be ensured, and the product production yield can be improved. In actual application, the aluminum product is rotated in a clockwise direction at a speed of 300 for 5 minutes. Visually check that there is no residual water on the surface of the product, and pay attention to safety and environmental protection issues.

[0064] S9, dyeing with gradient color: soaking the hanger with the anode product in the gradient color dyeing solution, the dye components of the gradient color dyeing solution are metal composite color powder and dextrin;

[0065] In step S9, the dye components of the gradient dye solution include 30% metal composite color powder, 68.5% dextrin, and a sustained-release agent; the metal composite color powder includes two dyes, one dye (Ono 102) has a concentration of 2.5-3.5 g / L, and the optimal concentration is 3.0 g / L; the concentration of the other dye (Ono 507) is 0.8-1.2 g / L, and the optimal concentration is 1.0 g / L; the dextrin is 5-chloro-2-methyl-3-ketone with a proportion of 1.5%; the sustained-release agent is Na2SO4 with a concentration of 1 g / L; the pH value of the base color dye solution is 5-7.

[0066] S10, sealing: placing the hanger with the anode product in the sealing solution, so that the anode product is completely immersed in the sealing solution for sealing treatment;

[0067] In step S10, the sealing solution contains 75% nickel acetate, 5% sodium acetate and 20% chelating agent; the temperature of the sealing solution is 95±3°C; the immersion time of the anode product is 2400S; the concentration of the sealing solution is 10-12g / L, and the optimal concentration is 11g / L; the pH value of the sealing solution is 5.5-6.0.

[0068] S11, drying: drying the anode product.

[0069] like Figures 2 to 4 As shown, the two-color gradient characteristics of specific aluminum alloy products are:

[0070] Aluminum alloy two-color gradient refers to the color of the product surface slowly and naturally transitioning from light to dark or from one color to another. Two-color gradient methods include linear gradient, radial gradient, angle gradient, etc.

[0071] Implementation process:

[0072] The aluminum alloy two-color gradient first renders a target base color on the product surface, adds a dry water process, and then uses special equipment to rely on servo control to control the workpiece in different dyeing tanks. According to the needs, different speeds are set to slowly rise and fall to achieve different dyeing times, realizing a new gradient color effect with a natural transition of different colors from light to dark.

[0073] In the process of gradual dyeing of the surface of the anode product, different solution concentrations and components are used, which can achieve, for example, Figure 4 Gradient effect.

[0074] like Figure 2 and 3 As shown, the gradient ratio is:

[0075] The gradient scale size is from the starting point of the bottom of the product, the 0%-5% area is blue + purple as the base color area, the 5%-30% area is the two-color superimposed purple gradient transition area, and the 30%-100% is the blue pure color area.

[0076] like Figure 4 As shown, aluminum alloy oxidation: is a surface treatment technology that improves and enhances the performance of materials by forming a dense aluminum oxide film on the surface of aluminum or aluminum alloy products. This film layer has special properties such as protection, decoration, insulation, and wear resistance.

[0077] Aluminum alloy dyeing: also known as electrochemical coloring, is a process in which the dye molecules penetrate into the pores of the oxide film through electrolysis after the aluminum alloy surface has been anodized, forming an oxide film dye layer with color and decorative effects. Anodic dyeing can enrich the appearance color of aluminum alloy products and improve the aesthetics and added value of the products.

[0078] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described or replace them in a similar manner, but will not deviate from the spirit of the present invention or exceed the defined scope. Although the present invention is described and described in detail in the drawings and the foregoing description, such descriptions and descriptions are considered to be illustrative or exemplary rather than restrictive. It should be understood that within the scope of the following claims, changes and modifications may be made by a person of ordinary skill. Specifically, the present invention encompasses additional embodiments having any combination of features from the above-mentioned different embodiments. With respect to the use of the expression "generally" or "substantially", this patent application should be understood to disclose that these features and values ​​are also fully satisfied, i.e., there is no aforementioned characterization as "generally" or "substantially".

Claims

1. A process for gradual dyeing of the surface of an anode product, characterized in that: The following steps are involved: S1. Pre-treatment: including hanging, degreasing, neutralization and chemical polishing; S2. Oxidation: Place the hanger containing the anode product into the oxidation solution, so that the anode product is completely immersed in the oxidation solution for oxidation treatment; S3, dyeing the base color: soaking the hanger with the anode product in the base color dye solution, the dye components of the base color dye solution are metal composite color powder and dextrin; S4, rinsing: After the anode product has been dyed to reach a predetermined color difference value L, the anode product is subjected to multiple ultrapure water rinsing processes; S5, quick drying: put the rinsed anode product and the hanger into the centrifugal drying device, start the drying device to rotate at high speed, so that the residual water on the surface of the anode product is quickly dried during the rotation process; S6, dyeing with gradient color: soaking the hanger with the anode product in the gradient color dyeing solution, the dye components of the gradient color dyeing solution are metal composite color powder and dextrin; S7, sealing: placing the hanger with the anode product into the sealing solution, so that the anode product is completely immersed in the sealing solution for sealing treatment; S8, drying: drying the anode product.

2. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: Degreasing in step S1: placing the hanger with the anode product into the degreasing solution, and completely immersing the anode product in the degreasing solution for degreasing treatment; the degreasing solution comprises 5% sodium silicate, 10% chelating agent, 15% surfactant, 65% water, and 5% corrosion inhibitor; the concentration of the degreasing solution is 60±5g / L, the solution temperature is 60±2°C, and the immersion time of the anode product is 180±30s.

3. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: Neutralization in step S1: Place the hanger containing the anode product into the neutralization solution, and immerse the anode product completely in the neutralization solution for neutralization treatment; the neutralization solution is nitric acid, the concentration of the neutralization solution is 300-400g / L, and the immersion time of the anode product is 120±60S.

4. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: Chemical polishing in step S1: placing a hanger containing anode products into a chemical polishing solution, so that the anode products are completely immersed in the chemical polishing solution for chemical polishing treatment; the chemical polishing solution is a mixture of nitric acid and phosphoric acid, the solution concentration of H3PO4 in the chemical polishing solution is 1200±100g / L, the solution concentration of H2S04 is 240±30g / L, the specific gravity of the chemical polishing solution is 1.770-1.85, and the concentration of aluminum ions produced by the chemical polishing solution for chemical polishing of aluminum products is 10-30g / L.

5. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: In step S2, the oxidizing solution is sulfuric acid, and the solution components of the oxidizing solution include H2S04 concentration of 200±10g / L and Al3+ concentration of 0.5-15g / L; the temperature of the oxidizing solution is 19±1°C; the power-on voltage of the oxidizing solution is 15.0±0.5V; and the immersion time of the anode product is 2600±500s.

6. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: In step S3, the dye components of the base color dye solution include 30% metal composite color powder, 68.5% dextrin, and a sustained-release agent; the metal composite color powder includes two dyes, one dye has a concentration of 0.4-0.6g / L, and the other dye has a concentration of 0.01-0.02g / L; the dextrin is 5-chloro-2-methyl-3-ketone with a proportion of 1.5%; the sustained-release agent is Na2SO4 with a concentration of 1g / L; the pH value of the base color dye solution is 5-6.

7. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: In step S4, a color difference value L / a / b is predetermined, wherein L is 78 to 79.8; a is -106 to -11.1; b: -21.06~-22.06; the number of ultrapure water rinses is 3 times.

8. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: In step S5, the centrifugal drying device includes a drying drum and a centrifugal motor, the centrifugal motor is driven and connected to the drying drum, the centrifugal motor includes a rotor, a stator, a casing and an end cover, the rotor is disc-shaped, a support bearing is arranged at the center of the rotor, the rotor rotates relative to the stator, and the stator has a cylindrical casing. In step S5, the specific steps of quickly drying water include: a. Preparation stage: Check whether the centrifugal drying device is intact and ensure that it can operate normally; prepare the work area and ensure that it is clean and tidy to avoid contamination of the product; b. Loading products: Load the products onto the fixture and ensure that the products are fixed and stable and will not fall off or shift during the drying process; c. Drying operation: Place the hanger and the products on it into the spin-drying drum, and ensure that the hanger is firmly connected to the platform of the spin-drying drum; start the centrifugal motor to drive the spin-drying drum to rotate around the center line.

9. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: In step S6, the dye components of the gradient dye solution include 30% metal composite color powder, 68.5% dextrin, and a sustained-release agent; the metal composite color powder includes two dyes, one dye has a concentration of 2.5-3.5 g / L, and the other dye has a concentration of 0.8-1.2 g / L; the dextrin is 5-chloro-2-methyl-3-ketone with a proportion of 1.5%; the sustained-release agent is Na2SO4 with a concentration of 1 g / L; the pH value of the base color dye solution is 5-7.

10. The process for gradual dyeing of the surface of an anode product according to claim 1, characterized in that: In step S7, the sealing solution contains 75% nickel acetate, 5% sodium acetate and 20% chelating agent; the temperature of the sealing solution is 95±3°C; the immersion time of the anode product is 2400S; the concentration of the sealing solution is 10-12g / L; and the pH value of the sealing solution is 5.5-6.0.