A kind of anti-pollution high desalination reverse osmosis membrane and preparation method thereof
By using α-aldehyde-ω-carboxy polyethylene glycol to the chemical bond link between the polyamide layer and the PVA layer, a stable protective layer was formed, and the polyamide composite film pollution was solved through multiple dissolution-freezing and sonication treatment and The problem of desalination performance has achieved efficient anti-pollution and high desalination effects.
Patent Information
- Application Number
- CN202411329002.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-24
AI Technical Summary
Polyamide composite reverse osmosis membranes are easily contaminated during use, resulting in smaller membrane pore size, reduced clogging and desalination performance, and insufficient adhesion of existing PVA-coated protective layer, resulting in decreased anti-pollution performance and desalination rate.
Alpha-aldehyde-ω-carboxylic polyethylene glycol is used as a bridge compound, and the polyamide layer and PVA layer are connected through chemical bonds to form a stable protective layer, and the cross-linking degree of the PVA layer is improved through multiple dissolution-freezing treatment. , combined with sonication treatment to enhance the reaction of the membrane with the solution.
It significantly improves the anti-pollution and oxidation resistance of the polyamide reverse osmosis membrane, enhances the desalination rate of the membrane, reduces the cleaning cost and pollution risk, and extends the service life of the membrane.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of reverse osmosis composite membranes, and more specifically to a pollution-resistant high-desalination reverse osmosis membrane and a preparation method thereof. Background Art
[0002] Reverse osmosis technology is an advanced and energy-saving separation technology. Its principle is to separate the solute from the solvent in the solution under a pressure higher than the osmotic pressure of the solution by means of the selective interception of a semipermeable membrane that allows only water to pass through but not other substances. The separation characteristics of the reverse osmosis membrane can effectively remove impurities such as dissolved salts, colloids, organic matter, bacteria, and microorganisms in the water. It has the advantages of low energy consumption, no pollution, advanced technology, and simple operation and maintenance. Among them, polyamide composite reverse osmosis membranes have received widespread attention and use due to their excellent physical and chemical stability.
[0003] However, since the birth of reverse osmosis technology, the pollution and oxidative degradation of polyamide composite reverse osmosis membranes have always been the bottleneck restricting the promotion and development of this technology. The adsorption and deposition of pollutants on the membrane surface and in the membrane pores cause the membrane pore size to become smaller and clogged; in addition, pollutants are difficult to clean after adhering to the membrane surface, and the membrane flux will still decrease to a large extent after cleaning. At the same time, the active chlorine antibacterial agent added during the pretreatment of the influent will also oxidize the polyamide cortex, significantly reducing the desalination performance of the membrane material.
[0004] In order to solve the above problems, the method adopted in the prior art is to perform surface post-treatment on the reverse osmosis membrane to form a surface protective layer. Polyvinyl alcohol (PVA) has a strong hydrophilicity because it contains a large number of hydroxyl groups in its molecular structure. After being coated on the polyamide layer, it can increase the hydrophilicity of the membrane surface, thereby enhancing its anti-pollution ability. It is one of the most common reverse osmosis membrane polyamide surface coating protective layers.
[0005] At present, PVA is usually coated on the surface of the polyamide layer by physical coating. Due to its weak adhesion to the surface of the reverse osmosis membrane, the PVA layer will gradually fall off during the operation of the reverse osmosis membrane, causing the anti-pollution performance of the reverse osmosis membrane to gradually lose. At the same time, since the PVA layer is electrically neutral and the polyamide layer is usually negatively charged, the surface charging effect of the polyamide reverse osmosis composite membrane coated with PVA will be weakened, resulting in a certain decrease in the desalination rate. Summary of the invention
[0006] In view of this, the object of the present invention is to provide a reverse osmosis membrane with high pollution resistance and desalination rate and a preparation method thereof. The product obtained by the preparation method provided by the present invention has good pollution resistance, oxidation resistance and high desalination rate.
[0007] The present invention provides a method for preparing a pollution-resistant high-desalination reverse osmosis membrane, comprising the following steps:
[0008] a) gelling the polyvinyl alcohol aqueous solution, and then adding α-aldehyde-ω-carboxyl polyethylene glycol to dissolve the solution to obtain a grafting post-treatment solution;
[0009] b) coating the polysulfone support layer with an aqueous phase liquid, and coating the polysulfone support layer with an oil phase solution after solidification and drying to form a polyamide ultra-thin separation layer, thereby obtaining a nascent polyamide reverse osmosis membrane; and then immersing the nascent polyamide reverse osmosis membrane in the grafting post-treatment solution obtained in step a), performing ultrasonic treatment, and taking out and draining to obtain a pollution-resistant and high-desalination reverse osmosis membrane.
[0010] Preferably, the concentration of the polyvinyl alcohol aqueous solution in step a) is 5 g / L-30 g / L; and the mass ratio of the α-aldehyde-ω-carboxyl polyethylene glycol to polyvinyl alcohol is (5-30):(1-5).
[0011] Preferably, the gelling treatment in step a) is carried out by multiple dissolution-freezing, specifically:
[0012] The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C to 90°C, then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and finally cooled at room temperature and α-aldehyde-ω-carboxyl polyethylene glycol is added to dissolve to obtain a grafting post-treatment solution;
[0013] or,
[0014] The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C to 90°C, then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and finally cooled at room temperature and α-aldehyde-ω-carboxyl polyethylene glycol is added to dissolve to obtain a grafting post-treatment solution;
[0015] or,
[0016] The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C~90°C, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, finally cooled at room temperature, added with α-aldehyde-ω-carboxyl polyethylene glycol to dissolve, and obtained a grafting post-treatment solution.
[0017] Preferably, the preparation method of the aqueous phase liquid in step b) is specifically:
[0018] One of aromatic, aliphatic or alicyclic multifunctional amines is selected and dissolved in water, and its weight concentration in the aqueous solution is 0.5% to 5%. After it is completely dissolved, a surfactant accounting for 0.5% to 2% of the weight of the aqueous solution and a polar solvent accounting for 3% to 10% of the weight of the aqueous solution are added to the aqueous solution. After stirring evenly, sodium hydroxide is added to adjust the pH value of the solution to between 7 and 9 to obtain an aqueous phase liquid.
[0019] Preferably, the aromatic, aliphatic or alicyclic polyfunctional amine includes one or more of m-phenylenediamine, ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, N-(2-hydroxyethyl)ethylenediamine, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, diethylenetriamine, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, mesitylenetriamine, piperazine, and 4-aminomethylpiperazine;
[0020] The surfactant is sodium dodecylbenzene sulfonate and / or sodium lauryl sulfate;
[0021] The polar solvent is dimethyl sulfoxide and / or N-methylpyrrolidone.
[0022] Preferably, the preparation method of the oil phase solution in step b) is specifically as follows:
[0023] One or more of aromatic, aliphatic or alicyclic multifunctional acyl halides are selected and dissolved in one of aliphatic hydrocarbons, cycloaliphatic hydrocarbons and aromatic hydrocarbons containing 4 to 12 carbon atoms at a ratio of 0.05% to 0.3% by weight of the total solution, and after stirring and dissolving, an oil phase solution is obtained.
[0024] Preferably, the aromatic, aliphatic or alicyclic multifunctional acyl halide is trimesoyl chloride.
[0025] Preferably, the drying method in step b) is oven drying; the oven drying temperature is 60°C to 80°C.
[0026] Preferably, the immersion temperature in step b) is 20° C. to 60° C.; and the ultrasonic treatment time is 10 min to 120 min.
[0027] The present invention also provides a pollution-resistant high-desalination reverse osmosis membrane, which is prepared by the preparation method described in the above technical solution.
[0028] The invention provides a high-desalination anti-pollution reverse osmosis membrane and a preparation method thereof. The preparation method comprises the following steps: a) gelling a polyvinyl alcohol aqueous solution, adding α-aldehyde-ω-carboxyl polyethylene glycol to dissolve, and obtaining a grafting post-treatment solution; b) coating a water phase liquid on a polysulfone support layer, and then coating an oil phase solution after solidification and drying to form a polyamide ultra-thin separation layer to obtain a nascent polyamide reverse osmosis membrane; and then immersing the nascent polyamide reverse osmosis membrane in the grafting post-treatment solution obtained in step a), performing ultrasonic treatment, taking out and draining, and obtaining a high-desalination anti-pollution reverse osmosis membrane. Compared with the prior art, the present invention aims to solve the technical problems that physically coated PVA is easy to fall off and the desalination rate will decrease to a certain extent after PVA coating. A bifunctional polymer α-aldehyde-ω-carboxyl polyethylene glycol that can react with the residual amino groups in the polyamide layer and the hydroxyl groups in the PVA is used as a bridging compound, so that the polyamide and the PVA are linked by chemical bonds. This makes it difficult for the PVA layer on the surface of the polyamide reverse osmosis composite membrane to fall off during use, thereby having better anti-pollution performance.
[0029] At the same time, the present invention uses a freeze-thaw method to gel the PVA to a certain extent when preparing the PVA coating solution, that is, it has a higher degree of cross-linking, which is beneficial to improving the desalination rate of the polyamide reverse osmosis composite membrane.
[0030] In addition, in the present invention, when the α-aldehyde-ω-carboxyl polyethylene glycol is treated, ultrasonic treatment is used to make it more fully bonded to the polyamide layer and the PVA layer.
[0031] Finally, the preparation method provided by the present invention has a simple process, easy-to-operate steps, mild and easy-to-control conditions, and has broad application prospects. DETAILED DESCRIPTION
[0032] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] The present invention provides a method for preparing a pollution-resistant high-desalination reverse osmosis membrane, comprising the following steps:
[0034] a) gelling the polyvinyl alcohol aqueous solution, and then adding α-aldehyde-ω-carboxyl polyethylene glycol to dissolve the solution to obtain a grafting post-treatment solution;
[0035] b) coating the polysulfone support layer with an aqueous phase liquid, and coating the polysulfone support layer with an oil phase solution after solidification and drying to form a polyamide ultra-thin separation layer, thereby obtaining a nascent polyamide reverse osmosis membrane; and then immersing the nascent polyamide reverse osmosis membrane in the grafting post-treatment solution obtained in step a), performing ultrasonic treatment, and taking out and draining to obtain a pollution-resistant and high-desalination reverse osmosis membrane.
[0036] At present, due to the inherent hydrophobicity of the surface of polyamide reverse osmosis composite membrane, various pollutants in the influent water are easily adhered to the membrane surface during application, resulting in the attenuation of membrane flux and the increase of energy consumption. The membrane assembly must be physically or chemically cleaned to remove the contamination layer to a certain extent. The traditional cleaning method is costly and ineffective, and may even cause the membrane separation performance to decline or even fail. At the same time, the active chlorine antibacterial agent added during the influent pretreatment process will also oxidize the polyamide cortex, resulting in a significant decrease in the membrane desalination rate, which limits the promotion and application of reverse osmosis composite membrane separation technology. Therefore, improving the anti-pollution and desalination rate of reverse osmosis membranes is of great theoretical and practical significance.
[0037] The present invention aims to solve the technical problems that physically coated PVA is easy to fall off, resulting in a decrease in its anti-pollution performance, and that the desalination rate will decrease to a certain extent after PVA coating. The present invention uses a bifunctional polymer α-aldehyde-ω-carboxyl polyethylene glycol that can react with the amino groups remaining in the polyamide layer and the hydroxyl groups in the PVA at the same time as a bridging compound, so that the polyamide and the PVA are linked through chemical bonds. This makes it difficult for the PVA layer on the surface of the polyamide reverse osmosis composite membrane to fall off during use, thereby having better anti-pollution performance.
[0038] The invention firstly performs gelation treatment on a polyvinyl alcohol aqueous solution, and then adds alpha-aldehyde-omega-carboxyl polyethylene glycol to dissolve the solution, so as to obtain a grafting post-treatment solution.
[0039] The present invention has no special restrictions on the type and source of the polyvinyl alcohol (PVA), and commercially available PVA known to those skilled in the art may be used, such as one or more of PVA-17-99, PVA-20-99, PVA-17-88, PVA-17-92, PVA-117, PVA-105, PVA-124, PVA-217, PVA-205, and PVA-224.
[0040] In the present invention, the concentration of the polyvinyl alcohol aqueous solution is preferably 5 g / L~30 g / L, more preferably 10 g / L~20 g / L; the mass ratio of the α-aldehyde-ω-carboxyl polyethylene glycol to polyvinyl alcohol is preferably (5~30):(1~5), more preferably (10~20):(1~5); on this basis, the concentration of the α-aldehyde-ω-carboxyl polyethylene glycol is 1 g / L~5 g / L.
[0041] In the present invention, the gelation treatment is preferably carried out by multiple dissolution-freezing. The present invention treats the PVA solution by multiple dissolution-freezing, which enhances the hydrogen bonding and van der Waals forces between PVA molecules, and the PVA layer has a higher degree of physical crosslinking. The gelation treatment process is preferably specifically as follows:
[0042] The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C to 90°C, then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and finally cooled at room temperature and α-aldehyde-ω-carboxyl polyethylene glycol is added to dissolve to obtain a grafting post-treatment solution;
[0043] or,
[0044] The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C to 90°C, then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and finally cooled at room temperature and α-aldehyde-ω-carboxyl polyethylene glycol is added to dissolve to obtain a grafting post-treatment solution;
[0045] or,
[0046] The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C~90°C, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, finally cooled at room temperature, added with α-aldehyde-ω-carboxyl polyethylene glycol to dissolve, and obtained a grafting post-treatment solution.
[0047] After obtaining the grafting post-treatment solution, the present invention coats an aqueous phase liquid on the polysulfone support layer, solidifies it, and then coats it with an oil phase solution for drying to form a polyamide ultra-thin separation layer to obtain a nascent polyamide reverse osmosis membrane; then the nascent polyamide reverse osmosis membrane is immersed in the obtained grafting post-treatment solution, subjected to ultrasonic treatment, taken out and drained to obtain a pollution-resistant and high-desalination reverse osmosis membrane.
[0048] The present invention has no special limitation on the source of the polysulfone support layer, and any commercially available product or self-made product known to those skilled in the art can be used.
[0049] In the present invention, the preparation method of the aqueous phase liquid is preferably as follows:
[0050] One of aromatic, aliphatic or alicyclic multifunctional amines is selected and dissolved in water, and its weight concentration in the aqueous solution is 0.5% to 5%. After it is completely dissolved, a surfactant accounting for 0.5% to 2% of the weight of the aqueous solution and a polar solvent accounting for 3% to 10% of the weight of the aqueous solution are added to the aqueous solution. After stirring evenly, sodium hydroxide is added to adjust the pH value of the solution to between 7 and 9 to obtain an aqueous phase liquid.
[0051] In the present invention, the aromatic, aliphatic or alicyclic polyfunctional amine preferably includes one or more of m-phenylenediamine, ethylenediamine, propylenediamine, butylenediamine, hexylenediamine, N-(2-hydroxyethyl)ethylenediamine, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, diethylenetriamine, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, s-phenylenediamine, piperazine, and 4-aminomethylpiperazine, and m-phenylenediamine is more preferred; the surfactant is preferably sodium dodecylbenzenesulfonate and / or sodium lauryl sulfate, and is more preferred; the polar solvent is preferably dimethyl sulfoxide and / or N-methylpyrrolidone, and is more preferred N-methylpyrrolidone. The present invention has no special restrictions on the sources of the aromatic, aliphatic or alicyclic polyfunctional amines, surfactants, and polar solvents, and commercially available products known to those skilled in the art can be used.
[0052] In the present invention, the preparation method of the oil phase solution is preferably as follows:
[0053] One or more of aromatic, aliphatic or alicyclic multifunctional acyl halides are selected and dissolved in one of aliphatic hydrocarbons, cycloaliphatic hydrocarbons and aromatic hydrocarbons containing 4 to 12 carbon atoms at a ratio of 0.05% to 0.3% by weight of the total solution, and after stirring and dissolving, an oil phase solution is obtained.
[0054] In the present invention, the aromatic, aliphatic or alicyclic polyfunctional acyl halide is preferably trimesoyl chloride. The present invention has no particular restrictions on the sources of the aromatic, aliphatic or alicyclic polyfunctional acyl halide and the aliphatic hydrocarbon, cycloaliphatic hydrocarbon and aromatic hydrocarbon containing 4 to 12 carbon atoms, and commercially available products well known to those skilled in the art can be used.
[0055] In the present invention, the drying method is preferably oven drying; the temperature of the oven drying is preferably 60°C to 80°C.
[0056] The key to the present invention is to immerse the nascent polyamide reverse osmosis membrane into the obtained grafting post-treatment solution; α-aldehyde-ω-carboxyl polyethylene glycol is added to the above grafting post-treatment solution, and the present invention uses α-aldehyde-ω-carboxyl polyethylene glycol as a grafting polymer, the aldehyde group at one end of the polymer can react with the hydroxyl group in PVA, and the carboxyl group at the other end can react with the amino group on the polyamide layer, so that the PVA is linked to the polyamide layer through a chemical bond, and the PVA forms a protective layer on the surface of the polyamide layer that is not easy to fall off, which can greatly improve the anti-pollution and anti-oxidation capabilities of the polyamide reverse osmosis membrane; at the same time, the α-aldehyde-ω-carboxyl polyethylene glycol used in the present invention as a grafting polymer itself also has strong hydrophilicity, which can improve the hydrophilicity of the surface of the polyamide layer, thereby improving its anti-pollution ability.
[0057] In the present invention, the immersion temperature is preferably 20°C to 60°C.
[0058] In the present invention, the ultrasonic treatment time is preferably 10 min to 120 min. The ultrasonic treatment is used to allow the α-aldehyde-ω-carboxyl polyethylene glycol to be more fully used in bridging the polyamide layer and the PVA layer.
[0059] The present invention also provides a high-desalination anti-pollution reverse osmosis membrane, which is prepared by the preparation method described in the above technical solution. The high-desalination anti-pollution reverse osmosis membrane provided by the present invention is formed by a polyamide separation layer, which is treated with a grafting post-treatment solution, so that the polyamide separation layer has good anti-pollution, anti-oxidation and high desalination rate, and is easy to clean.
[0060] The invention provides a high-desalination anti-pollution reverse osmosis membrane and a preparation method thereof. The preparation method comprises the following steps: a) gelling a polyvinyl alcohol aqueous solution, adding α-aldehyde-ω-carboxyl polyethylene glycol to dissolve, and obtaining a grafting post-treatment solution; b) coating a water phase liquid on a polysulfone support layer, and then coating an oil phase solution after solidification and drying to form a polyamide ultra-thin separation layer to obtain a nascent polyamide reverse osmosis membrane; and then immersing the nascent polyamide reverse osmosis membrane in the grafting post-treatment solution obtained in step a), performing ultrasonic treatment, taking out and draining, and obtaining a high-desalination anti-pollution reverse osmosis membrane. Compared with the prior art, the present invention aims to solve the technical problems that physically coated PVA is easy to fall off and the desalination rate will decrease to a certain extent after PVA coating. A bifunctional polymer α-aldehyde-ω-carboxyl polyethylene glycol that can react with the residual amino groups in the polyamide layer and the hydroxyl groups in the PVA is used as a bridging compound, so that the polyamide and the PVA are linked by chemical bonds. This makes it difficult for the PVA layer on the surface of the polyamide reverse osmosis composite membrane to fall off during use, thereby having better anti-pollution performance.
[0061] At the same time, the present invention uses a freeze-thaw method to gel the PVA to a certain extent when preparing the PVA coating solution, that is, it has a higher degree of cross-linking, which is beneficial to improving the desalination rate of the polyamide reverse osmosis composite membrane.
[0062] In addition, in the present invention, when the α-aldehyde-ω-carboxyl polyethylene glycol is treated, ultrasonic treatment is used to make it more fully bonded to the polyamide layer and the PVA layer.
[0063] Finally, the preparation method provided by the present invention has a simple process, easy-to-operate steps, mild and easy-to-control conditions, and has broad application prospects.
[0064] The present invention adopts a self-made porous polysulfone support layer bottom membrane, on which an aqueous phase liquid is first coated, and then an oil phase solution is coated, and the two phases are subjected to interfacial polymerization to obtain a nascent aromatic polyamide reverse osmosis membrane, and then the nascent membrane is subjected to grafting post-treatment to finally obtain a pollution-resistant and high-desalination polyamide reverse osmosis membrane. In order to further illustrate the present invention, the following examples are described in detail. The raw materials used in the following examples of the present invention are all commercially available.
[0065] Comparative Example 1
[0066] A method for producing a pollution-resistant and high-desalination polyamide reverse osmosis membrane is as follows:
[0067] (1) Preparation of aqueous phase liquid: Add 30g of m-phenylenediamine, 3g of sodium dodecylbenzene sulfonate, and 20g of N-methylpyrrolidone to 947g of water, adjust the pH value to 8.5-9 with sodium hydroxide, and stir evenly to obtain an aqueous phase solution.
[0068] (2) Preparation of oil phase solution: Dissolve 3 g of trimesoyl chloride in 997 g of Isopar G and stir well to obtain an oil phase solution.
[0069] (3) First, an aqueous solution is coated on the polysulfone support layer. After removing excess solution on the surface and air-drying, an oil solution is coated thereon. After removing excess oil solution on the surface, the support layer is dried in an oven at 70°C ± 3°C to form a polyamide ultra-thin separation layer, thereby obtaining a primary polyamide reverse osmosis membrane.
[0070] Performance test: 2000ppm sodium chloride aqueous solution was filtered for 30min at 1.55MPa, 25℃ and membrane flow rate of 1.1L / min, and the initial flux and desalination rate of the nascent polyamide reverse osmosis membrane were tested; under the same operating conditions, the test aqueous solution was replaced with 1000ppm bovine serum albumin solution and lysozyme solution, respectively. The bovine serum albumin solution was first filtered for 150min, and then the lysozyme solution was filtered for 90min, a total of 240min, and then the test solution was replaced with 2000ppm sodium chloride aqueous solution. 2000ppm sodium chloride aqueous solution was filtered for 30min at 1.55MPa, 25℃ and membrane flow rate of 1.1L / min, and the flux and desalination rate of the nascent polyamide reverse osmosis membrane after pollution were tested. All test results are shown in Table 1.
[0071] Comparative Example 2
[0072] A method for producing a pollution-resistant and high-desalination polyamide reverse osmosis membrane is as follows:
[0073] (1) Preparation of aqueous phase: same as Comparative Example 1.
[0074] (2) Preparation of oil phase solution: same as Comparative Example 1.
[0075] (3) Preparation of post-grafting treatment solution: PVA was heated and dissolved at a temperature of 80°C ± 3°C at a concentration of 15 g / L, and then cooled at room temperature to obtain a post-grafting treatment solution.
[0076] (4) First, an aqueous solution is coated on the polysulfone support layer, and after removing excess solution on the surface and air drying, an oil phase solution is coated thereon, and after removing excess oil phase solution on the surface, the support layer is dried in an oven at 70°C±3°C to form a polyamide ultra-thin separation layer, thereby obtaining a nascent polyamide reverse osmosis membrane; then, the nascent polyamide reverse osmosis membrane is immersed in a grafting post-treatment solution at 40°C±5°C, ultrasonically treated (40kHz±5kHz) for 65 minutes, and then removed to remove excess post-treatment solution. After draining, a pollution-resistant and high-desalination polyamide reverse osmosis membrane is obtained.
[0077] Performance test: 2000ppm sodium chloride aqueous solution was filtered for 30min at 1.55MPa, 25℃ and membrane flow rate of 1.1L / min, and the initial flux and desalination rate of the anti-pollution and high-desalination polyamide reverse osmosis membrane were tested; under the same operating conditions, the test aqueous solution was replaced with 1000ppm bovine serum albumin solution and lysozyme solution, respectively. The bovine serum albumin solution was first filtered for 150min, and then the lysozyme solution was filtered for 90min, a total of 240min, and then the test solution was replaced with 2000ppm sodium chloride aqueous solution. 2000ppm sodium chloride aqueous solution was filtered for 30min at 1.55MPa, 25℃ and membrane flow rate of 1.1L / min, and the post-pollution flux and desalination rate of the anti-pollution and high-desalination polyamide reverse osmosis membrane were tested. All test results are shown in Table 1.
[0078] Comparative Example 3
[0079] A method for producing a pollution-resistant and high-desalination polyamide reverse osmosis membrane is as follows:
[0080] (1) Preparation of aqueous phase: same as Comparative Example 1.
[0081] (2) Preparation of oil phase solution: same as Comparative Example 1.
[0082] (3) Preparation of post-grafting treatment solution: Heat and dissolve acetylated polyvinyl alcohol at a concentration of 15 g / L at a temperature of 80°C ± 3°C, and cool at room temperature to obtain a post-grafting treatment solution.
[0083] (4) First, an aqueous solution is coated on the polysulfone support layer, and after removing the excess solution on the surface and air drying, an oil phase solution is coated thereon, and after removing the excess oil phase solution on the surface, the support layer is placed in a 70°C±3°C oven for drying to form a polyamide ultra-thin separation layer, thereby obtaining a nascent polyamide reverse osmosis membrane; then, the nascent polyamide reverse osmosis membrane is immersed in a grafting post-treatment solution at 40°C±5°C, subjected to ultrasonic treatment (40kHz±5kHz) for 65 minutes, and the excess post-treatment solution is removed and drained to obtain a pollution-resistant and high-desalination polyamide reverse osmosis membrane.
[0084] Performance test: Same as Comparative Example 2; all test results are shown in Table 1.
[0085] Example 1
[0086] A method for producing a pollution-resistant and high-desalination polyamide reverse osmosis membrane is as follows:
[0087] (1) Preparation of aqueous phase: same as Comparative Example 1.
[0088] (2) Preparation of oil phase solution: same as Comparative Example 1.
[0089] (3) Preparation of post-grafting treatment solution: Heat and dissolve PVA at a concentration of 15 g / L at 80°C ± 3°C, then cool at -13 to -12°C, heat and dissolve again at 80°C ± 3°C, then cool at -13 to -12°C, heat and dissolve again at 80°C ± 3°C, cool at room temperature, add 1 g / L of α-aldehyde-ω-carboxyl polyethylene glycol to obtain a post-grafting treatment solution.
[0090] (4) First, an aqueous solution is coated on the polysulfone support layer, and after removing excess solution on the surface and air drying, an oil phase solution is coated thereon, and after removing excess oil phase solution on the surface, the support layer is dried in an oven at 70°C±3°C to form a polyamide ultra-thin separation layer, thereby obtaining a nascent polyamide reverse osmosis membrane; then, the nascent polyamide reverse osmosis membrane is immersed in a grafting post-treatment solution at 40°C±5°C, ultrasonically treated (40kHz±5kHz) for 65 minutes, and then removed to remove excess post-treatment solution. After draining, a pollution-resistant and high-desalination polyamide reverse osmosis membrane is obtained.
[0091] Performance test: Same as comparative example 2; all test results are shown in Table 1.
[0092] Example 2
[0093] The preparation method provided in Example 1 was used, except that: in step (3), 3 g / L of α-aldehyde-ω-carboxyl polyethylene glycol was added to dissolve to obtain a grafting post-treatment solution.
[0094] Performance test: Same as Comparative Example 2; all test results are shown in Table 1.
[0095] Example 3
[0096] The preparation method provided in Example 1 was used, except that: in step (3), 5 g / L of α-aldehyde-ω-carboxyl polyethylene glycol was added to dissolve to obtain a grafting post-treatment solution.
[0097] Performance test: Same as Comparative Example 2; all test results are shown in Table 1.
[0098] Example 4
[0099] The preparation method provided in Example 1 was adopted, except that: in step (3), PVA was heated and dissolved at a temperature of 80°C±3°C at a concentration of 15 g / L, then cooled at a temperature of -13 to -12°C, and after cooling, heated and dissolved again at a temperature of 80°C±3°C, and then cooled at room temperature and 3 g / L of α-aldehyde-ω-carboxyl polyethylene glycol was added to obtain a grafting post-treatment solution.
[0100] Performance test: Same as Comparative Example 2; all test results are shown in Table 1.
[0101] Example 5
[0102] The preparation method provided in Example 1 is adopted, except that: in step (3), PVA is heated and dissolved at a temperature of 80°C±3°C at a concentration of 15 g / L, and then cooled at a temperature of -13 to -12°C, and then heated and dissolved again at a temperature of 80°C±3°C after cooling, and then cooled at a temperature of -13 to -12°C, and then heated and dissolved again at a temperature of 80°C±3°C after cooling, and then cooled at a temperature of -13 to -12°C, and then heated and dissolved again at a temperature of 80°C±3°C, and then cooled at room temperature, and then 3 g / L of α-aldehyde-ω-carboxyl polyethylene glycol is added to obtain a grafting post-treatment solution.
[0103] Performance test: Same as Comparative Example 2; all test results are shown in Table 1.
[0104] Table 1 Product anti-pollution performance test data
[0105]
[0106] Among them, the flux attenuation rate after pollution = (1-flux after pollution / initial flux) × 100%; the desalination rate attenuation rate after pollution = (1-desalination rate after pollution / initial desalination rate) × 100%.
[0107] Principle: (1) One end of α-aldehyde-ω-carboxyl polyethylene glycol is an aldehyde group, which can react chemically with the hydroxyl group on PVA, and the other end of the carboxyl group can react chemically with the residual amino group on polyamide. This allows the polyamide layer and the PVA layer to be connected by chemical bonds during PVA coating, thereby forming a stable anti-fouling layer on the surface of the polyamide layer; (2) After repeated dissolution and freezing, PVA has a physical cross-linking degree due to its hydrogen bonding and van der Waals force. This can be used to After the frozen PVA is coated on the polyamide layer, the desalination rate of the polyamide reverse osmosis composite membrane can be improved due to the increase in its physical cross-linking degree; (3) α-aldehyde-ω-carboxyl polyethylene glycol also increases the overall cross-linking degree of the polyamide reverse osmosis composite membrane when bridging the polyamide layer and the PVA layer, thereby improving its desalination rate; (4) α-aldehyde-ω-carboxyl polyethylene glycol itself is also a hydrophilic polymer. After it is grafted onto the surface of the polyamide layer, it can also increase the hydrophilicity of the polyamide layer surface and thus improve its anti-pollution ability.
[0108] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing a pollution-resistant high-desalination reverse osmosis membrane, comprising the following steps: a) gelling the polyvinyl alcohol aqueous solution, and then adding α-aldehyde-ω-carboxyl polyethylene glycol to dissolve the solution to obtain a grafting post-treatment solution; b) coating the polysulfone support layer with an aqueous phase liquid, and coating the polysulfone support layer with an oil phase solution after solidification and drying to form a polyamide ultra-thin separation layer, thereby obtaining a nascent polyamide reverse osmosis membrane; and then immersing the nascent polyamide reverse osmosis membrane in the grafting post-treatment solution obtained in step a), performing ultrasonic treatment, and taking out and draining to obtain a pollution-resistant and high-desalination reverse osmosis membrane.
2. The preparation method according to claim 1, characterized in that: The concentration of the polyvinyl alcohol aqueous solution in step a) is 5 g / L-30 g / L; the mass ratio of the α-aldehyde-ω-carboxyl polyethylene glycol to the polyvinyl alcohol is (5-30):(1-5).
3. The preparation method according to claim 1, characterized in that: The gelation treatment in step a) is carried out by multiple dissolution-freezing, specifically: The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C to 90°C, then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and finally cooled at room temperature and α-aldehyde-ω-carboxyl polyethylene glycol is added to dissolve to obtain a grafting post-treatment solution; or, The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C to 90°C, then cooled at -20°C to -5°C, and then heated to dissolve at 70°C to 90°C again after cooling, and finally cooled at room temperature and α-aldehyde-ω-carboxyl polyethylene glycol is added to dissolve to obtain a grafting post-treatment solution; or, The polyvinyl alcohol aqueous solution is heated to dissolve at 70°C~90°C, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, then cooled at -20°C~-5°C, heated to dissolve at 70°C~90°C again after cooling, finally cooled at room temperature, added with α-aldehyde-ω-carboxyl polyethylene glycol to dissolve, and obtained a grafting post-treatment solution.
4. The preparation method according to claim 1, characterized in that: The preparation method of the aqueous phase liquid in step b) is specifically as follows: One of aromatic, aliphatic or alicyclic multifunctional amines is selected and dissolved in water, and its weight concentration in the aqueous solution is 0.5% to 5%. After it is completely dissolved, a surfactant accounting for 0.5% to 2% of the weight of the aqueous solution and a polar solvent accounting for 3% to 10% of the weight of the aqueous solution are added to the aqueous solution. After stirring evenly, sodium hydroxide is added to adjust the pH value of the solution to between 7 and 9 to obtain an aqueous phase liquid.
5. The preparation method according to claim 4, characterized in that: The aromatic, aliphatic or alicyclic polyfunctional amines include one or more of m-phenylenediamine, ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, N-(2-hydroxyethyl)ethylenediamine, 1,2-diaminocyclohexane, 1,3-diaminocyclohexane, 1,4-diaminocyclohexane, diethylenetriamine, m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, s-phenylenediamine, piperazine, and 4-aminomethylpiperazine; The surfactant is sodium dodecylbenzene sulfonate and / or sodium lauryl sulfate; The polar solvent is dimethyl sulfoxide and / or N-methylpyrrolidone.
6. The preparation method according to claim 1, characterized in that: The preparation method of the oil phase solution in step b) is specifically as follows: One or more of aromatic, aliphatic or alicyclic multifunctional acyl halides are selected and dissolved in one of aliphatic hydrocarbons, cycloaliphatic hydrocarbons and aromatic hydrocarbons containing 4 to 12 carbon atoms at a ratio of 0.05% to 0.3% by weight of the total solution, and after stirring and dissolving, an oil phase solution is obtained.
7. The preparation method according to claim 6, characterized in that: The aromatic, aliphatic or alicyclic multifunctional acyl halide is trimesoyl chloride.
8. The preparation method according to claim 1, characterized in that: The drying method in step b) is oven drying; the oven drying temperature is 60°C to 80°C.
9. The preparation method according to claim 1, characterized in that: In step b), the immersion temperature is 20° C. to 60° C.; and the ultrasonic treatment time is 10 min to 120 min.
10. A reverse osmosis membrane with high pollution resistance and desalination, characterized in that: The method is prepared by any one of claims 1 to 9.