Paper tube for winding silk and preparation method of paper tube
By using a combined structure of kraft paper, enhanced light-curing glue and a transparent porous film in the textile paper tube, and using ultraviolet curing, the problem of poor composite effect between the inner core and the base paper in the existing technology is solved, and high compressive strength is achieved and paper tube preparation with simplified processes.
Patent Information
- Application Number
- CN202410895268.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
AI Technical Summary
The material properties of the inner core of existing textile paper tubes result in poor hot-melt adhesive bonding effects between the inner core and the base paper, requiring the use of two types of glue and multiple processes, which is cumbersome.
It adopts a combined structure of outer layer of kraft paper, middle layer of enhanced light-curing glue and inner layer of transparent porous film. The glue is cured through ultraviolet irradiation, simplifying the process.
It improves the composite strength of the paper tube, simplifies the process flow, reduces the use of glue, and forms a paper tube with high compressive strength and not easy to deform.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a paper tube for winding yarns and a preparation method thereof. Background Art
[0002] Paper tubes are widely used in the textile industry. They can be used to wind yarn, which is beneficial for the storage and transportation of yarn.
[0003] Invention patent application CN116533601A discloses a preparation process for textile paper tubes, which includes base paper selection, base paper quality inspection, base pad preparation, felt preparation, inner core preparation, brushing to remove impurities, corona treatment, composite process, glue coating, paper tube forming and other processes.
[0004] However, its inner core is made of a base pad and felt needle-punched together, and it also needs to be brushed to remove impurities. Due to the material properties of the inner core, the effect of compounding the inner core and the base paper with hot-melt adhesive needs to be further improved; and it still needs to be coated with reinforced latex on the composite substrate and then dried. Since two types of glue are used twice, the entire process is more cumbersome.
[0005] Based on this, the present invention designs a paper tube for winding wire and a preparation method thereof to solve the above problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a paper tube for winding wire and a preparation method thereof.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A paper tube for winding yarn, comprising an outer layer of kraft paper, a middle layer of enhanced light-curing glue and an inner layer of a transparent porous film;
[0009] The enhanced light-curing glue comprises the following raw materials in parts by weight: 30-45 parts of epoxy soybean oil or 25-36 parts of cardanol, 5-11 parts or 13-20 parts of acrylate, 3-6 parts of diphenylmethane diisocyanate (MDI), 1-3 parts of phenyltrimethylammonium hydroxide, 3-5 parts of hydroxypropyl methacrylate, 13-15 parts of hexahydrophthalic anhydride, and 0.6-1.3 parts of photoinitiator;
[0010] The transparent porous membrane comprises the following raw materials in parts by weight: 5 to 8 parts of glass fiber, 22 to 30 parts of polyvinylidene fluoride, 3 to 7 parts of polylactic acid, 1.3 to 3 parts of gelatinized starch, and 0.4 to 1 part of silicon dioxide;
[0011] Furthermore, the thickness ratio of the kraft paper, the transparent porous film, and the enhanced light-curing glue is 10.6-15.3:2.2-2.5:1.
[0012] Furthermore, the mass ratio of epoxidized soybean oil to acrylate is 30-45:5-11.
[0013] Furthermore, the mass ratio of cardanol to acrylate is 25-36:13-20.
[0014] A method for preparing a paper tube for winding wire comprises the following steps:
[0015] 1. Preparation of enhanced light-curing glue
[0016] Epoxidized soybean oil or cardanol reacts with acrylate at 105-119° C. until the acid value of the reaction solution remains unchanged, diphenylmethane diisocyanate and phenyltrimethylammonium hydroxide are added, and the reaction is continued for 3-5 hours to obtain a combination component 1;
[0017] Hydroxypropyl methacrylate and hexahydrophthalic anhydride are subjected to esterification reaction at 108-112° C. for 5-8 hours to obtain component 2; component 1, component 2 and a photoinitiator are stirred and reacted at 25-30° C. for 10-15 minutes to obtain an enhanced light-curing adhesive;
[0018] 2. Preparation of transparent porous membrane
[0019] The glass fiber, polyvinylidene fluoride, polylactic acid, gelatinized starch and silicon dioxide are melted and mixed, and a film is extruded through an extruder, and then cooled to 50-55°C;
[0020] Then, the film is stretched horizontally in the left and right directions and in the front and back directions by using a stretching device;
[0021] Then, the film is introduced into a tentering machine for processing to obtain a transparent porous film;
[0022] 3. Use a glue coating device to coat the enhanced light-curing glue on the outer layer of kraft paper;
[0023] Fourth, a composite device is used to roll-compound the kraft paper and the inner transparent porous film to enhance the penetration of the light-curing glue into the pores of the transparent porous film;
[0024] 5. Use the tube rolling equipment to roll the tube to obtain the paper tube, and then irradiate the inside and both sides of the paper tube with ultraviolet light for curing;
[0025] 6. Cut the pipe and discharge the material.
[0026] Furthermore, in step 2, the extrusion temperature range is controlled to be 195-212°C.
[0027] Furthermore, in step 2, the film is stretched horizontally in left-right and front-back directions by a stretching device, with a left-right stretching ratio of 3.2 to 4.0 times and a front-back stretching ratio of 3.5 to 4.2 times; the stretching temperature is 143 to 155°C.
[0028] Furthermore, in step 2, a tentering machine is introduced, the transverse tension is adjusted to 280-300N, the temperature is adjusted to 135-140°C, and the film is treated under these conditions for 3-5 minutes to obtain a transparent porous film.
[0029] Compared with the prior art, the present invention has the following beneficial effects:
[0030] The present invention compounds the kraft paper of the outer layer and the transparent porous film of the inner layer through the enhanced light-curing glue of the middle layer, obtains the paper tube after the tube rolling operation, and then cures the inside and both sides of the paper tube by ultraviolet irradiation, so as to obtain the paper tube with high composite strength. One and one enhanced light-curing glue is used, and drying is not required, so the process flow is simpler; the glue can be cured quickly, and the formed paper roll has high compressive strength, does not peel, is not easy to deform, and is widely used. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Embodiment 1
[0033] In some embodiments, a method for preparing a paper tube for winding wire comprises the following steps:
[0034] 1. Preparation of enhanced light-curing glue
[0035] Weigh the following raw materials: 30 g of epoxidized soybean oil, 11 g of acrylate, 3 g of diphenylmethane diisocyanate (MDI), 3 g of phenyltrimethylammonium hydroxide, 3 g of hydroxypropyl methacrylate, 5 g of hexahydrophthalic anhydride, and 0.6 g of photoinitiator;
[0036] Epoxidized soybean oil and acrylate are reacted at 105°C until the acid value of the reaction solution remains unchanged, diphenylmethane diisocyanate and phenyltrimethylammonium hydroxide are added, and the reaction is continued for 5 hours to obtain a combination component 1;
[0037] Hydroxypropyl methacrylate and hexahydrophthalic anhydride are subjected to esterification reaction at 108° C. for 8 hours to obtain component 2; component 1, component 2 and a photoinitiator are stirred and reacted at 25° C. for 15 minutes to obtain an enhanced light-curing adhesive;
[0038] 2. Preparation of transparent porous membrane
[0039] Weigh the following raw materials: 5 g of glass fiber, 30 g of polyvinylidene fluoride, 3 g of polylactic acid, 3 g of gelatinized starch, and 0.4 g of silicon dioxide;
[0040] The glass fiber, polyvinylidene fluoride, polylactic acid, gelatinized starch and silicon dioxide are melted and mixed, and a film is extruded through an extruder, and then cooled to 50°C; the extrusion temperature range is controlled to be 195-212°C;
[0041] Then, the film was stretched horizontally in the left and right directions and in the front and back directions by a stretching device, with the stretching ratio of 3.2 times for the left and right directions and 3.5 times for the front and back directions; the stretching temperature was 155°C;
[0042] Then, the film was introduced into a tenter, the transverse tension was adjusted to 280 N, the temperature was adjusted to 140° C., and the film was treated under this condition for 3 minutes to obtain a transparent porous film;
[0043] 3. Use a glue coating device to coat the enhanced light-curing glue on the outer layer of kraft paper;
[0044] Fourth, a composite device is used to roll-compound the kraft paper and the inner transparent porous film to enhance the penetration of the light-curing glue into the pores of the transparent porous film;
[0045] 5. Use the tube rolling equipment to roll the tube to obtain the paper tube, and then irradiate the inside and both sides of the paper tube with ultraviolet light for curing;
[0046] 6. Cut the pipe and discharge the material.
[0047] The thickness ratio of the outer layer of kraft paper, the inner layer of transparent porous film and the middle layer of enhanced light-curing glue is 10.6:2.5:1.
[0048] Embodiment 2
[0049] In some embodiments, a method for preparing a paper tube for winding wire comprises the following steps:
[0050] 1. Preparation of enhanced light-curing glue
[0051] Weigh the following raw materials: 45 g of epoxy soybean oil, 5 g of acrylate, 6 g of diphenylmethane diisocyanate (MDI), 1 g of phenyltrimethylammonium hydroxide, 5 g of hydroxypropyl methacrylate, 13 g of hexahydrophthalic anhydride, and 1.3 g of photoinitiator;
[0052] Epoxidized soybean oil and acrylate are reacted at 119° C. until the acid value of the reaction solution remains unchanged, diphenylmethane diisocyanate and phenyltrimethylammonium hydroxide are added, and the reaction is continued for 3 hours to obtain a combination component 1;
[0053] Hydroxypropyl methacrylate and hexahydrophthalic anhydride are subjected to esterification reaction at 112° C. for 5 hours to obtain component 2; component 1, component 2 and a photoinitiator are stirred and reacted at 30° C. for 10 minutes to obtain an enhanced light-curing adhesive;
[0054] 2. Preparation of transparent porous membrane
[0055] Weigh the following raw materials: 8 g of glass fiber, 22 g of polyvinylidene fluoride, 7 g of polylactic acid, 1.3 g of gelatinized starch, and 1 g of silicon dioxide;
[0056] The glass fiber, polyvinylidene fluoride, polylactic acid, gelatinized starch and silicon dioxide are melted and mixed, and a film is extruded through an extruder, and then cooled to 55°C; the extrusion temperature range is controlled to be 195-212°C;
[0057] Then, the film was stretched horizontally in the left-right and front-back directions by a stretching device, with a stretching ratio of 4.0 times for the left and right and 4.2 times for the front-back. The stretching temperature was 143°C.
[0058] Then, the film was introduced into a tentering machine, the transverse tension was adjusted to 300 N, the temperature was adjusted to 135° C., and the film was treated under this condition for 5 minutes to obtain a transparent porous film.
[0059] 3. Use a glue coating device to coat the enhanced light-curing glue on the outer layer of kraft paper;
[0060] Fourth, a composite device is used to roll-compound the kraft paper and the inner transparent porous film to enhance the penetration of the light-curing glue into the pores of the transparent porous film;
[0061] 5. Use the tube rolling equipment to roll the tube to obtain the paper tube, and then irradiate the inside and both sides of the paper tube with ultraviolet light for curing;
[0062] 6. Cut the pipe and discharge the material.
[0063] The thickness ratio of the outer layer of kraft paper, the inner layer of transparent porous film and the middle layer of enhanced light-curing glue is 15.3:2.2:1.
[0064] Embodiment 3
[0065] In some embodiments, a method for preparing a paper tube for winding wire comprises the following steps:
[0066] 1. Preparation of enhanced light-curing glue
[0067] Weigh the following raw materials: 40 g of epoxy soybean oil, 8 g of acrylate, 5.5 g of diphenylmethane diisocyanate (MDI), 1.3 g of phenyltrimethylammonium hydroxide, 3.9 g of hydroxypropyl methacrylate, 14.5 g of hexahydrophthalic anhydride, and 1 g of photoinitiator;
[0068] Epoxidized soybean oil and acrylate were reacted at 110°C until the acid value of the reaction solution remained unchanged, diphenylmethane diisocyanate and phenyltrimethylammonium hydroxide were added, and the reaction was continued for 3.6 hours to obtain a combination component 1;
[0069] Hydroxypropyl methacrylate and hexahydrophthalic anhydride are subjected to esterification reaction at 109° C. for 6.2 hours to obtain component 2; component 1, component 2 and a photoinitiator are stirred and reacted at 28° C. for 12 minutes to obtain an enhanced light-curing adhesive;
[0070] 2. Preparation of transparent porous membrane
[0071] Weigh the following raw materials: 6.6 g of glass fiber, 24.3 g of polyvinylidene fluoride, 5.4 g of polylactic acid, 1.6 g of gelatinized starch, and 0.6 g of silicon dioxide;
[0072] The glass fiber, polyvinylidene fluoride, polylactic acid, gelatinized starch and silicon dioxide are melted and mixed, and a film is extruded through an extruder, and then cooled to 52°C; the extrusion temperature range is controlled to be 195-212°C;
[0073] Then, the film was stretched horizontally in the left and right directions and in the front and back directions by using a stretching device, with the left and right stretching ratio being 4.0 times and the front and back stretching ratio being 4 times; the stretching temperature was 145°C;
[0074] Then, the film was introduced into a tenter, the transverse tension was adjusted to 285 N, the temperature was adjusted to 136° C., and the film was treated under this condition for 4 minutes to obtain a transparent porous film.
[0075] 3. Use a glue coating device to coat the enhanced light-curing glue on the outer layer of kraft paper;
[0076] Fourth, a composite device is used to roll-compound the kraft paper and the inner transparent porous film to enhance the penetration of the light-curing glue into the pores of the transparent porous film;
[0077] 5. Use the tube rolling equipment to roll the tube to obtain the paper tube, and then irradiate the inside and both sides of the paper tube with ultraviolet light for curing;
[0078] 6. Cut the pipe and discharge the material.
[0079] The thickness ratio of the outer layer of kraft paper, the inner layer of transparent porous film and the middle layer of enhanced light-curing glue is 13.3:2.3:1.
[0080] Example 4
[0081] The difference from Example 1 is that in step 1:
[0082] 30 g of epoxidized soybean oil was replaced with 25 g of cardanol.
[0083] Example 5
[0084] The difference from Example 1 is that in step 1:
[0085] 30 g of epoxidized soybean oil was replaced with 36 g of cardanol.
[0086] Example 6
[0087] The difference from Example 1 is that in step 1:
[0088] 30 g of epoxidized soybean oil was replaced with 32 g of cardanol.
[0089] The present invention compounds the kraft paper of the outer layer and the transparent porous film of the inner layer through the enhanced light-curing glue of the middle layer, obtains the paper tube after the tube rolling operation, and then cures the inside and both sides of the paper tube by ultraviolet irradiation, so as to obtain the paper tube with high composite strength. One and one enhanced light-curing glue is used, and drying is not required, so the process flow is simpler; the glue can be cured quickly, and the formed paper roll has high compressive strength, does not peel, is not easy to deform, and is widely used.
[0090] The paper tube with a thickness of 1 cm and a length of 1 cm prepared in Example 1 was subjected to a compression test using a paper tube compression strength tester, and the result showed that the compressive strength was 45.8 kg.
[0091] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A paper tube for winding wire, characterized in that it comprises an outer layer of kraft paper, a middle layer of enhanced light-curing glue and an inner layer of a transparent porous film; The enhanced light-curing glue comprises the following raw materials in parts by weight: 30-45 parts of epoxy soybean oil or 25-36 parts of cardanol, 5-11 parts or 13-20 parts of acrylate, 3-6 parts of diphenylmethane diisocyanate (MDI), 1-3 parts of phenyltrimethylammonium hydroxide, 3-5 parts of hydroxypropyl methacrylate, 13-15 parts of hexahydrophthalic anhydride, and 0.6-1.3 parts of photoinitiator; The transparent porous film comprises the following raw materials in parts by weight: 5 to 8 parts of glass fiber, 22 to 30 parts of polyvinylidene fluoride, 3 to 7 parts of polylactic acid, 1.3 to 3 parts of gelatinized starch, and 0.4 to 1 part of silicon dioxide.
2. The paper tube for winding wire according to claim 1, characterized in that: The thickness ratio of the kraft paper, the transparent porous film and the enhanced light-curing glue is 10.6-15.3:2.2-2.5:
1.
3. The paper tube for winding wire according to claim 2, characterized in that: The mass ratio of epoxidized soybean oil to acrylate is 30-45:5-11.
4. The paper tube for winding wire according to claim 3, characterized in that: The mass ratio of cardanol to acrylate is 25-36:13-20.
5. A method for preparing a paper tube for winding wire according to claim 4, characterized in that: The following steps are involved:
1. Preparation of enhanced light-curing glue Epoxidized soybean oil or cardanol reacts with acrylate at 105-119° C. until the acid value of the reaction solution remains unchanged, diphenylmethane diisocyanate and phenyltrimethylammonium hydroxide are added, and the reaction is continued for 3-5 hours to obtain a combination component 1; Hydroxypropyl methacrylate and hexahydrophthalic anhydride are subjected to esterification reaction at 108-112° C. for 5-8 hours to obtain component 2; component 1, component 2 and a photoinitiator are stirred and reacted at 25-30° C. for 10-15 minutes to obtain an enhanced light-curing adhesive; 2. Preparation of transparent porous membrane The glass fiber, polyvinylidene fluoride, polylactic acid, gelatinized starch and silicon dioxide are melted and mixed, and a film is extruded through an extruder, and then cooled to 50-55°C; Then, the film is stretched horizontally in the left and right directions and in the front and back directions by using a stretching device; Then, the film is introduced into a tentering machine for processing to obtain a transparent porous film; 3. Use a glue coating device to coat the enhanced light-curing glue on the outer layer of kraft paper; Fourth, a composite device is used to roll-compound the kraft paper and the inner transparent porous film to enhance the penetration of the light-curing glue into the pores of the transparent porous film; 5. Use the tube rolling equipment to roll the tube to obtain the paper tube, and then irradiate the inside and both sides of the paper tube with ultraviolet light for curing; 6. Cut the pipe and discharge the material.
6. The method for preparing a paper tube for winding wire according to claim 5, characterized in that: In step 2, the extrusion temperature range is controlled to be 195-212°C.
7. The method for preparing a paper tube for winding wire according to claim 6, characterized in that: In step 2, the film is stretched horizontally in left-right and front-back directions by a stretching device, with a left-right stretching ratio of 3.2 to 4.0 times and a front-back stretching ratio of 3.5 to 4.2 times; the stretching temperature is 143 to 155°C.
8. The method for preparing a paper tube for winding wire according to claim 7, characterized in that: In step 2, the film is introduced into a tentering machine, the transverse tension is adjusted to 280-300N and the temperature is adjusted to 135-140°C, and the film is treated under these conditions for 3-5 minutes to obtain a transparent porous film.