Composite anhydride modified UV (ultraviolet) photocurable epoxy acrylate as well as preparation method and application thereof
By compounding glutaric anhydride, maleic anhydride and epoxy resin, combined with hydroxyethyl acrylate, a composite anhydride-modified UV-curable epoxy acrylate is prepared, which solves the problem of insufficient hardness and flexibility of existing coatings and achieves It achieves high hardness, flexibility and chemical resistance, and reduces production costs and operation difficulty.
Patent Information
- Application Number
- CN202410979280.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-22
AI Technical Summary
Existing UV-cured epoxy acrylate coatings have deficiencies in hardness, flexibility and chemical resistance, and traditional methods of increasing toughness will increase the molecular weight and viscosity of the resin, resulting in unstable storage and reduced hardness of the coating film.
Using glutaric anhydride, maleic anhydride, phthalic anhydride and hydroxyethyl acrylate to react, combined with epoxy resin and catalyst, composite anhydride-modified UV-curable epoxy acrylate is prepared through a one-step method, and the reaction conditions and formulations are controlled. To improve the hardness, flexibility and impact resistance of the coating film.
It achieves high hardness, excellent flexibility and impact resistance, while reducing the viscosity and production cost of the resin. The chemical resistance of the coating film is significantly improved, and the process is simple and the operation difficulty is low.
Smart Images

Figure CN118852584A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of preparation of ultraviolet light-curing epoxy acrylate coatings, and in particular to composite acid anhydride-modified UV-curable epoxy acrylate and a preparation method and application thereof. Background Art
[0002] Ultraviolet (UV) curing technology refers to the process in which, under the irradiation of ultraviolet light, the photoinitiator in the system absorbs energy to produce free radicals or cations, which in turn triggers chemical reactions such as grafting, polymerization, and cross-linking of oligomers containing active groups and active diluents, thereby promoting the rapid curing of the substrate surface into a film. Different from existing traditional coatings such as solvent-based, water-based, and thermosetting, the advantages of UV curing technology are that the paint film cures quickly, does not require the use of solvents, is simple to operate, and the curing process is not easily affected by factors such as temperature and environment. As my country's industry gradually shifts towards green, environmentally friendly, energy-efficient, and intelligent directions, the industrial application of UV curing technology has developed rapidly.
[0003] Epoxy acrylate resin is the most commonly used UV light-curing resin, and bisphenol A epoxy acrylate is the fastest curing type in epoxy acrylate oligomers, and is also the most widely used type. Due to the presence of rigid benzene ring structure in the structure, UV-cured coating film is brittle and poor in flexibility, and weather resistance, light aging resistance and yellowing resistance are not good. To solve these defects, Chinese invention patent CN102295730A discloses a synthetic method of intramolecular toughening epoxy vinyl ester resin, first using long-chain saturated dibasic acid and flexible diol reaction to obtain terminal carboxyl long-chain saturated dibasic acid monoester, and then reacting with epoxy resin and unsaturated monocarboxylic acid until the acid value is reduced to less than 10mgKOH / g. The method has the advantages of introducing flexible molecular chains on the resin main chain, thereby improving the toughness of the resin, and its disadvantage is that the introduction of dibasic acid monoesters will increase the molecular weight and viscosity of the resin, and the dosage is large, the resin viscosity increases, storage is unstable, and the coating hardness is reduced, and the toughening effect is poor. The patent application with publication number CN104558522A discloses a modification method of modified epoxy acrylate, which uses bisphenol A epoxy resin and 1,2-cyclohexanediol diglycidyl ether to react to generate modified epoxy resin. The synthesis method is to add the above two materials and catalyst to a reaction vessel, stir and heat to 80-90°C, gradually drip acrylic acid and inhibitor mixture within 0.5-1h, and then gradually heat until the acid value drops below 3.0mgKOH / g to obtain modified epoxy acrylate. Although this patent solves the problems of high resin viscosity, high film brittleness and poor flexibility, the patent actually achieves this goal by mixing 1,2-cyclohexanediol diglycidyl ether diacrylate into ordinary epoxy acrylic resin in a physical blending manner, which can easily reduce the hardness of the coating film. Therefore, the development of a modified epoxy acrylic resin with high hardness, high toughness and good flexibility is a technical problem that needs to be solved in this field. Summary of the invention
[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing a composite anhydride modified UV-curable epoxy acrylate, which is inexpensive, has low product cost, does not use any solvent in the reaction process, and reduces VOC emissions; the prepared epoxy acrylate has high hardness, excellent adhesion, flexibility, impact resistance and chemical resistance after being cured into a film.
[0005] Another object of the present invention is to provide a composite anhydride modified UV light-curable epoxy acrylate.
[0006] Another object of the present invention is to provide an application of the above-mentioned composite anhydride modified UV light-curable epoxy acrylate for preparing a coating, wherein the cured coating film has the characteristics of high hardness, excellent flexibility and impact resistance, chemical resistance, heat resistance and fast curing speed.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The present invention provides a method for preparing composite anhydride-modified UV-curable epoxy acrylate, comprising the following steps:
[0009] (1) Weigh the raw materials according to the following formula by weight:
[0010]
[0011] (2) stirring and heating glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin, part of the catalyst, and part of the polymerization inhibitor to 75° C. to 80° C. and keeping the temperature for 0.8 to 1.2 hours, then heating the mixture in stages, adding the remaining catalyst and the remaining polymerization inhibitor in batches, and finally heating the mixture to 115 to 125° C. and reacting the mixture for 4 to 5 hours to obtain a composite anhydride-modified UV-curable epoxy acrylate;
[0012] The weight of the partial catalyst is 55% to 65% of the total weight of the catalyst; the weight of the partial polymerization inhibitor is 55% to 65% of the total weight of the polymerization inhibitor.
[0013] Preferably, the epoxy resin is one of epoxy resins E51, E44, F44, F51, 170, 128, R-828, S-21, and BD-20.
[0014] Preferably, the catalyst is at least one of tetraethylammonium bromide, tetrabutylammonium bromide, N,N-dimethylbenzylamine and triphenylphosphine.
[0015] Preferably, the polymerization inhibitor is at least one of p-hydroxyanisole, p-benzoquinone, methylhydroquinone, hydroquinone, and 2,5-dimethylhydroquinone.
[0016] Preferably, the stepwise heating and batchwise addition of the remaining catalyst and the remaining polymerization inhibitor are specifically as follows:
[0017] Raise the temperature by 8-10°C every 0.8-1.2 hours; add the remaining catalyst and remaining inhibitor in 4-5 portions.
[0018] The present invention also provides a composite anhydride modified UV light-curable epoxy acrylate, which comprises, by weight:
[0019]
[0020] The invention also provides application of the composite anhydride modified UV light-curable epoxy acrylate for preparing coatings.
[0021] Preferably, the coating comprises 65 to 87 parts of composite anhydride-modified UV-curable epoxy acrylate, 10 to 30 parts of reactive diluent, and 3 to 5 parts of photoinitiator.
[0022] Preferably, the reactive diluent is one of tripropylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, hexanediol diacrylate and triethylene glycol diacrylate.
[0023] Preferably, the photoinitiator is at least one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and 1-hydroxycyclohexyl phenyl ketone.
[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0025] (1) The present invention introduces a vinyl monocarboxylic acid intermediate and a rigid benzene ring by compounding glutaric anhydride, maleic anhydride and phthalic anhydride and reacting them with hydroxyethyl acrylate to increase the crosslinking density of the UV-cured coating film, thereby increasing the hardness and chemical resistance of the modified epoxy acrylic resin product.
[0026] (2) The present invention combines glutaric anhydride, maleic anhydride and phthalic anhydride by compounding and reasonably limiting their ratio, thereby combining a rigid structure with a flexible long chain, and optimizing and improving the balance between high hardness, high flexibility and high impact resistance of the UV-cured coating.
[0027] (3) The UV-curable epoxy acrylate prepared by the one-step method of the present invention has a simple synthesis process, mild reaction conditions, low industrial operation difficulty, a wide source of raw materials and low prices, and a low resin preparation cost. The coating prepared by the resin can be directly applied to UV curing, and has the prospect of large-scale production in industry.
[0028] (4) The composite anhydride modified UV-curable epoxy acrylate of the present invention can be applied to many fields such as primer and topcoat, plastic paint and printing ink, and the coating has high crosslinking density, high hardness but good flexibility, and excellent chemical resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the infrared spectrum of the composite anhydride modified UV-curable epoxy acrylate in Example 1 of the present invention.
[0030] Figure 2 This is the H-NMR spectrum of the composite anhydride-modified UV-curable epoxy acrylate in Example 1 of the present invention.
[0031] Figure 3 This is the gel chromatogram of the composite anhydride modified UV-curable epoxy acrylate in Example 1 of the present invention.
[0032] Figure 4 Schematic diagram of the synthesis process of composite anhydride modified UV-curable epoxy acrylate in Example 1 of the present invention. DETAILED DESCRIPTION
[0033] The present invention will be further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.
[0034] The comparative example in each embodiment is that the EA resin produced by Beixin Carpoly Chemical Group Co., Ltd. replaces the modified epoxy acrylate of the present invention as the oligomer component of the UV-curing coating, and the other components and proportions are the same as those in the embodiment.
[0035] In the following examples, the properties of UV-curable resins and light-curable coatings are tested according to the following methods: the viscosity of the resin is measured using an NDJ-8 rotational viscometer according to GB / T21059-2007; the acid value of the resin is measured according to GB / T 6743-2008; the hardness of the coating is measured according to GB / T 6739-2006; the adhesion of the coating is measured according to GB-T 9286-1998; the water resistance of the coating is measured by a room temperature immersion method according to GB / T5209-1985; the alcohol resistance of the coating is measured according to GB / T 1763-79; the acid / alkali resistance of the coating is measured according to GB / T 9274-2009; the impact resistance of the coating is measured according to GB / T 20624.2-2006; and the flexibility of the coating is measured using a QTY-10A paint film bending tester according to GB / T 1731-1993.
[0036] Example 1
[0037] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 1:
[0038]
[0039] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0040] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0041] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: light yellow, transparent and clear in appearance; acid value is 2.7 mgKOH / g; viscosity is 124500 mPa·s.
[0042] (3) Preparation of UV curing coating:
[0043] The configuration composition of the UV curing coating is shown in Table 2 in parts by mass:
[0044]
[0045] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example coating 1 was compared with the same EA resin on the market. The coating performance is shown in Table 3.
[0046] (4) Table 3:
[0047]
[0048] As can be seen from Table 3, compared with the existing products, the composite anhydride modified UV-curable epoxy acrylate resin obtained by the present invention not only has a lower resin viscosity, but also has a moderate hardness of the obtained cured film, and not only has improved adhesion of the paint film, but also greatly improved flexibility and impact resistance, and at the same time has excellent chemical resistance.
[0049] Figure 1 This is the infrared spectrum of the composite anhydride modified UV-curable epoxy acrylate in Example 1. It can be seen from the figure that 910 cm -1 The peak of the epoxy group at 1719 cm -1The peak of ester bond appears at 3467cm -1 The peak attributable to hydroxyl group is enhanced at 1607 cm -1 The characteristic peak of carbon-carbon double bond appeared at 1760 cm-1, which proved the successful grafting of epoxy resin ring opening and carboxyl intermediate with acrylic acid. -1 、1850cm -1 The characteristic peak of the anhydride carbonyl group at indicates that the anhydride group also reacted during the process.
[0050] Figure 2 This is the H-NMR spectrum of the composite anhydride modified UV-curable epoxy acrylate in Example 1, the benzene ring proton peak on phthalic anhydride at 7.7-7.8ppm, 7.1ppm and 6.8ppm belong to the benzene ring proton peak on the epoxy resin, 5.9-6.3ppm belongs to the double bond proton peak of hydroxyethyl acrylate, the hydroxyl group generated by the esterification reaction of anhydride and hydroxyethyl acrylate is located at 5.4ppm, 4.8ppm is the double bond proton peak of maleic anhydride, and the methylene peaks on glutaric anhydride and hydroxyethyl acrylate are located at 3.7-4.5ppm. The above results prove that the anhydride, hydroxyethyl acrylate and acrylic acid are successfully grafted on E51.
[0051] Figure 3 This is the gel chromatogram of the composite anhydride modified UV-curable epoxy acrylate in Example 1. The data of the UV-curable epoxy acrylate synthesized in Example 1 can be obtained: the number average molecular weight (Mn) is 1282 g / mol, and the weight average molecular weight (Mw) is 1321 g / mol.
[0052] Figure 4 The reaction flow chart and molecular structure diagram in Example 1, wherein the composite acid anhydride reacts with hydroxyethyl acrylate to generate a carboxyl-containing intermediate, which then undergoes a ring-opening reaction with acrylic acid and epoxy resin E51. There are many types of acid anhydrides, and there are many possible molecular structures generated during the reaction.
[0053] Compared with comparative patent 1 (CN102295730A), the resin prepared by the present invention has low viscosity, can take into account both the hardness and flexibility of the coating film, and has low reaction temperature, simple process, and good storage stability of the resin. Compared with comparative patent 2 (CN104558522A), the resin prepared by the present invention has uniform components, can coordinate the contradiction between high coating film hardness and high toughness, and has low resin production cost and simple process.
[0054] Example 2
[0055] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 4:
[0056]
[0057]
[0058] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0059] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0060] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: light yellow, transparent and clear in appearance; acid value is 1.8 mgKOH / g; viscosity is 118350 mPa·s.
[0061] (3) Preparation of UV curing coating:
[0062] The configuration composition of the UV curing coating is shown in Table 5 in parts by mass:
[0063]
[0064] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 2 and the same EA resin on the market were compared, and the coating performance was tested and shown in Table 6.
[0065] (4) Table 6:
[0066]
[0067]
[0068] Example 3
[0069] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 7:
[0070]
[0071] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0072] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0073] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: light yellow, transparent and clear in appearance; acid value is 1.5 mgKOH / g; viscosity is 115600 mPa·s.
[0074] (3) Preparation of UV curing coating:
[0075] The configuration composition of the UV curing coating is shown in Table 8 below, in parts by mass:
[0076]
[0077] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 3 and the same EA resin on the market were compared, and the coating performance was tested and shown in Table 9.
[0078] (4) Table 9:
[0079]
[0080] Example 4
[0081] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 10:
[0082]
[0083] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0084] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0085] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: light yellow, transparent and clear in appearance; acid value is 2.5 mgKOH / g; viscosity is 143150 mPa·s.
[0086] (3) Preparation of UV curing coating:
[0087] The configuration composition of the UV curing coating is shown in Table 11 in parts by mass:
[0088]
[0089] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 4 was compared with the same EA resin on the market. The coating performance test is shown in Table 12.
[0090] (4) Table 12:
[0091]
[0092] Example 5
[0093] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 13:
[0094]
[0095] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0096] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0097] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: light yellow, transparent and clear in appearance; acid value is 2.7 mgKOH / g; viscosity is 138550 mPa·s.
[0098] (3) Preparation of UV curing coating:
[0099] The configuration composition of the UV curing coating is shown in Table 14 in parts by mass:
[0100]
[0101] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 5 and the same EA resin on the market were compared, and the coating performance was tested and shown in Table 15.
[0102] (4) Table 15:
[0103]
[0104]
[0105] Example 6
[0106] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 16:
[0107]
[0108] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0109] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0110] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: light yellow, transparent and clear in appearance; acid value is 1.9 mgKOH / g; viscosity is 134800 mPa·s.
[0111] (3) Preparation of UV curing coating:
[0112] The configuration composition of the UV curing coating is shown in Table 17 in parts by mass:
[0113]
[0114]
[0115] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 6 was compared with the same EA resin on the market. The coating performance test is shown in Table 18.
[0116] (4) Table 18:
[0117]
[0118] Example 7
[0119] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: A composite anhydride-modified UV-curable epoxy acrylate resin, the raw material formula weight percentage composition is shown in Table 19:
[0120]
[0121]
[0122] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0123] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0124] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: water white, transparent and clear appearance; acid value is 2.1 mgKOH / g; viscosity is 103850 mPa·s.
[0125] (3) Preparation of UV curing coating:
[0126] The configuration composition of the UV curing coating is shown in Table 20 below, in parts by mass:
[0127]
[0128] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 7 was compared with the same EA resin on the market. The coating performance is shown in Table 21.
[0129] (4) Table 21:
[0130]
[0131]
[0132] Example 8
[0133] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 22:
[0134]
[0135] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0136] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0137] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: water white, transparent and clear appearance; acid value is 1.6 mgKOH / g; viscosity is 101450 mPa·s.
[0138] (3) Preparation of UV curing coating:
[0139] The configuration composition of the UV curing coating is shown in Table 23 in parts by mass:
[0140]
[0141] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 8 was compared with the same EA resin on the market. The coating performance is shown in Table 24.
[0142] (4) Table 24:
[0143]
[0144] Example 9
[0145] (1) Preparation of composite anhydride-modified UV-curable epoxy acrylate: The composite anhydride-modified UV-curable epoxy acrylate resin of this embodiment has a raw material formula with a mass percentage composition as shown in Table 25:
[0146]
[0147] The preparation process of composite anhydride modified UV curable epoxy acrylate in this embodiment is as follows:
[0148] The above-mentioned glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin E51, tetraethylammonium bromide (accounting for 60%wt of the total amount of catalyst) and p-hydroxyanisole (the total amount is 60wt% of the total inhibitor) are added into a four-necked flask equipped with a stirring paddle, a thermometer and a condenser, and the temperature is raised to 75°C and kept warm for 1 hour; then 10wt% of tetraethylammonium bromide and p-hydroxyanisole are added every 1 hour, and the temperature is gradually raised to 83°C, 90°C, 97°C, 105°C, and finally raised to 120°C and kept warm for 4-5 hours. The acid value is measured to be lower than the theoretical value of 3.0mgKOH / g, the temperature is lowered and the material is discharged to obtain composite acid anhydride modified UV-curable epoxy acrylate.
[0149] (2) Physical and chemical properties of composite anhydride modified UV-curable epoxy resin: water white, transparent and clear appearance; acid value is 2.0 mgKOH / g; viscosity is 97650 mPa·s.
[0150] (3) Preparation of UV curing coating:
[0151] The configuration composition of the UV curing coating is shown in Table 26 in parts by mass:
[0152]
[0153] Add the above formula materials into the container and disperse at a low speed of 600r / min for 10-15min. After the paint is left to stand without bubbles, use a four-sided wet film applicator to apply the film on the wood board, glass board and tinplate respectively. The film thickness is 25±2μm and the power is 600mW / cm 2 , cured under a UV curing machine with a wavelength of 365nm, and the coating performance was tested. The coating performance is shown in the table below. The performance of Example 9 was compared with the same EA resin on the market. The coating performance was tested and shown in Table 27.
[0154] (4) Table 27:
[0155]
[0156] In the above embodiments, the epoxy resin may be one of epoxy resins E51, E44, F44, F51, 170, 128, R-828, S-21, and BD-20.
[0157] In the above embodiment, the catalyst may be at least one of tetraethylammonium bromide, tetrabutylammonium bromide, N,N-dimethylbenzylamine and triphenylphosphine.
[0158] In the above embodiments, the polymerization inhibitor is at least one of p-hydroxyanisole, p-benzoquinone, methylhydroquinone, hydroquinone, and 2,5-dimethylhydroquinone.
[0159] In the above embodiment, the active diluent may be one of tripropylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, hexanediol diacrylate and triethylene glycol diacrylate.
[0160] In the above embodiment, the photoinitiator may be at least one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, and 1-hydroxycyclohexyl phenyl ketone.
[0161] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A method for preparing a composite anhydride-modified UV-curable epoxy acrylate, characterized in that: The following steps are involved: (1) Weigh the raw materials according to the following formula by weight: (2) stirring and heating glutaric anhydride, maleic anhydride, phthalic anhydride, acrylic acid, hydroxyethyl acrylate, epoxy resin, part of the catalyst, and part of the polymerization inhibitor to 75° C. to 80° C. and keeping the temperature for 0.8 to 1.2 hours, then heating the mixture in stages, adding the remaining catalyst and the remaining polymerization inhibitor in batches, and finally heating the mixture to 115 to 125° C. and reacting the mixture for 4 to 5 hours to obtain a composite anhydride-modified UV-curable epoxy acrylate; The weight of the partial catalyst is 55% to 65% of the total weight of the catalyst; the weight of the partial polymerization inhibitor is 55% to 65% of the total weight of the polymerization inhibitor.
2. The method for preparing the composite anhydride modified UV-curable epoxy acrylate according to claim 1, characterized in that: The epoxy resin is one of epoxy resins E51, E44, F44, F51, 170, 128, R-828, S-21, and BD-20.
3. The method for preparing the composite anhydride modified UV-curable epoxy acrylate according to claim 1, characterized in that: The catalyst is at least one of tetraethylammonium bromide, tetrabutylammonium bromide, N,N-dimethylbenzylamine and triphenylphosphine.
4. The method for preparing the composite anhydride modified UV-curable epoxy acrylate according to claim 1, characterized in that: The polymerization inhibitor is at least one of p-hydroxyanisole, p-benzoquinone, methylhydroquinone, hydroquinone and 2,5-dimethylhydroquinone.
5. The method for preparing the composite anhydride modified UV-curable epoxy acrylate according to claim 1, characterized in that: The stepwise heating and batchwise addition of the remaining catalyst and the remaining polymerization inhibitor are specifically as follows: Raise the temperature by 8-10°C every 0.8-1.2 hours; add the remaining catalyst and remaining inhibitor in 4-5 portions.
6. A composite anhydride modified UV-curable epoxy acrylate, characterized in that: By weight, including:
7. The use of the composite anhydride modified UV-curable epoxy acrylate according to claim 6, characterized in that: Used to prepare coatings.
8. The use according to claim 7, characterized in that: The coating comprises, by weight, 65 to 87 parts of composite anhydride-modified UV-curable epoxy acrylate, 10 to 30 parts of reactive diluent, and 3 to 5 parts of photoinitiator.
9. The use according to claim 8, characterized in that: The active diluent is one of tripropylene glycol diacrylate, trimethylolpropane triacrylate, polyethylene glycol diacrylate, pentaerythritol triacrylate, dipentaerythritol pentaacrylate, hexanediol diacrylate and triethylene glycol diacrylate.
10. The use according to claim 8, characterized in that: The photoinitiator is at least one of 2-hydroxy-2-methyl-1-phenyl-1-propanone, diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide and 1-hydroxycyclohexyl phenyl ketone.
Citation Information
Patent Citations
Modified epoxy acrylic acid resin, preparation method and uses thereof
CN103087294A
Synthesizing method of modified epoxy acrylate resin
CN106188497A
Epoxy acrylate oligomer as well as preparation method and application thereof
CN109721708A
UV photocuring 3D printing resin as well as preparation method and application thereof
CN115819687A
Preparation method of ultraviolet curing flame-retardant epoxy acrylate and ultraviolet curing coating
CN115850658A