Transparent component and surface coating process thereof

By using a light-shading layer structure of hard coating, primer and color paint layer on transparent headlights, combined with hollow design and varnish layer, the problem of insufficient adhesion of spray paint is solved, and higher wear resistance is achieved and Aestheticity simplifies the spraying process and improves the durability and detection efficiency of the product.

CN118892977APending Publication Date: 2024-11-05SWELL MARUI GUANGZHOU AUTOMOBILE PARTS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991696.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Existing transparent car lights lack adhesion when spraying colored paint, resulting in durability and coverage uniformity problems, making it difficult to meet personalized appearance needs.

Method used

Adopt a light-shielding layer structure including hard coating, primer and color paint layer. Through the combination of hollow design and varnish layer, the adhesion and aesthetics are improved, and specific coating process steps and spray parameters are adopted, such as 45°- 90° spray gun angle and robot spray ensure coating uniformity and durability.

Benefits of technology

It significantly improves the wear resistance, light shielding ability and aesthetics of transparent components, enhances the adhesion between the colored paint layer and the hard coating layer, simplifies the spraying process, and improves the durability and detection efficiency of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118892977A_ABST
    Figure CN118892977A_ABST
Patent Text Reader

Abstract

The invention discloses a transparent component and a surface coating process thereof, and relates to the technical field of spraying, the transparent component comprises a base area and a light-transmitting area, the base area is located on the two sides of the light-transmitting area, and the light-transmitting area is covered with a hard coating which is used for protecting the surface of the transparent component and improving wear resistance; the light-transmitting area is provided with a colored paint area, the colored paint area is coated with a light-proof shading layer, and the shading layer comprises a bottom coating and a colored paint layer, so that the light shading capability is improved, the light-proof area is obviously formed, and the light effect of the lamp when the lamp is lightened is improved; the base coating is located between the hard coating and the colored paint layer, the base coating is beneficial to improving the adhesive force between the colored paint layer and the hard coating, the colored paint area is provided with a plurality of hollowed-out parts arranged at intervals, light can penetrate through the hollowed-out parts, and therefore the function of improving the attractiveness is achieved. The coating process comprises the steps of hard coating, shielding, prime coating, colored paint coating, laser etching, varnish coating and the like which are sequentially carried out, the steps can be simplified, and the efficiency and the attractive effect can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of spraying, and in particular to a transparent component and a surface coating process thereof. Background Art

[0002] With the rapid development of the automobile market, the personalized development of automobiles has become more and more prominent, and the diversified characteristics of various parts have become more and more prominent. In order to adapt to the young consumer group, the pursuit of personalized aesthetics in automobiles has gradually formed. Therefore, the personalized development of the front face of the car, including the shape and appearance of the headlights, has been continuously promoted. At present, the transparent headlights are generally coated with hard coating to improve the wear resistance and UV resistance of the lamps. However, when spraying the color paint on the headlights, it is easy to cause insufficient durability due to insufficient adhesion, and it is easy to cause uneven coverage during the spraying process. Summary of the invention

[0003] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a transparent component and a surface coating process thereof, which can improve the convenience of operation and the detection efficiency.

[0004] A transparent component according to an embodiment of the first aspect of the present invention is used in a lamp, comprising:

[0005] The substrate includes a base area and a light-transmitting area. The base area is located on both sides of the light-transmitting area. The light-transmitting area is covered with a hard coating layer. The light-transmitting area is provided with a colored paint area. The colored paint area is coated with an opaque shading layer. The shading layer includes a primer layer and a colored paint layer. The primer layer is located between the hard coating layer and the colored paint layer. The colored paint area has a plurality of hollow portions arranged at intervals, and the hollow portions can transmit light.

[0006] A transparent component according to an embodiment of the first aspect of the present invention is used on a lamp and has at least the following beneficial effects: the embodiment is provided with a substrate, the substrate includes a base area and a light-transmitting area, the base areas are located on both sides of the light-transmitting area, the light-transmitting area is covered with a hard coating layer, so as to protect the surface of the transparent component and improve the wear resistance; the light-transmitting area is provided with a colored paint area, the colored paint area is coated with an opaque shading layer, the shading layer includes a primer layer and a colored paint layer, which helps to improve the shading ability, significantly forms an opaque area, and improves the lighting effect of the lamp when it is lit; the primer layer is located between the hard coating layer and the colored paint layer, the primer layer helps to improve the adhesion between the colored paint layer and the hard coating layer, the colored paint area has a plurality of hollow portions arranged at intervals, the hollow portions can transmit light, so as to achieve the function of improving the aesthetics.

[0007] According to an embodiment of the first aspect of the present invention, the light-transmitting area further includes a transparent area located on one side of the color paint area, and the transparent area covers the periphery of the color paint area.

[0008] According to an embodiment of the first aspect of the present invention, a clear varnish layer is coated on the outer side of the color varnish layer away from the substrate.

[0009] According to an embodiment of the first aspect of the present invention, the substrate includes a front side and a back side, and the light shielding layer and the hard coating layer are located on the front side.

[0010] According to an embodiment of the first aspect of the present invention, the hard coating layer has a thickness of 90 μm-180 μm.

[0011] According to an embodiment of the second aspect of the present invention, a surface coating process is provided, which is applied to the above-mentioned transparent component and comprises the following steps:

[0012] Step 1: Hard coating, applying a hard coating on the front surface;

[0013] Step 2: Masking: paste masking paper on the transparent area on the front, and paste masking film on the back and base area;

[0014] Step 3: Primer coating: spray the primer on the front side covered with the hard coating to improve the bonding strength between the color paint layer and the hard coating;

[0015] Step 4: Color paint coating, spraying a color paint layer on the front side covered with the base coat;

[0016] Step 5: Laser engraving: laser engrave the color paint layer and carve a hollow part in the light-shielding layer;

[0017] Step 6: Varnish coating: spray a layer of varnish on the front side of the substrate.

[0018] The surface coating process according to the second aspect of the present invention has at least the following beneficial effects:

[0019] The process includes the steps of hard coating, masking, primer coating, color paint coating, laser engraving and clear coating. Before color paint coating, primer coating is applied on the hard coating layer to cover a layer of primer coating, which helps to improve the bonding strength between the color paint layer and the hard coating layer and improve the durability of the color paint layer. Masking is performed before primer coating and color paint layer coating to prevent the shading layer from covering other parts that need to be light-permeable and to improve the convenience of subsequent spraying process. Laser engraving after color paint coating helps to accurately control the pattern of the hollow part, improve the aesthetics and simplify the masking operation. Clear coating after laser engraving helps to further improve the protection of the substrate and its coating and improve the durability and aesthetics.

[0020] According to an embodiment of the second aspect of the present invention, the hard coating layer is cured after the hard coating layer is applied, and the curing is achieved by irradiating the hard coating layer with ultraviolet rays at a temperature of 40° C.-60° C.

[0021] According to an embodiment of the second aspect of the present invention, the base coating is sprayed with a spray gun, and the angle between the spray gun and the front surface during spraying is 45°-90°.

[0022] According to an embodiment of the second aspect of the present invention, the spraying speed of the primer coating ranges from 25 square meters to 55 square meters per hour, and the spraying pressure is controlled between 0.6 MPa and 2.0 MPa.

[0023] According to an embodiment of the second aspect of the present invention, a robot is used for automatic spraying of color paint, wherein the line speed during the spraying process is 30 to 120 meters per minute, and baking and curing are required after spraying is completed, the curing temperature is at least 80°C, and the baking time is at least 30 minutes.

[0024] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:

[0026] Figure 1 An isometric view of a transparent component in an embodiment of the first aspect of the present invention;

[0027] Figure 2 is a cross-sectional view of a transparent component in an embodiment of the first aspect of the present invention;

[0028] Figure 3 Schematic diagram of various coatings on a substrate in an embodiment of the first aspect of the present invention.

[0029] Reference numerals:

[0030] Base 100; base area 101; light-transmitting area 102; color paint area 103; transparent area 104; hollow part 105; front side 106; back side 107;

[0031] Hard coating layer 110; base coating layer 111; color paint layer 112; clear coating layer 113. DETAILED DESCRIPTION

[0032] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0033] In the description of the present invention, it should be understood that descriptions involving orientations, such as up, down, front, back, left, right, etc., and orientations or positional relationships indicated are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0034] In the description of the present invention, "several" means one or more, "more" means more than two, "greater than", "less than", "exceed" etc. are understood as not including the number itself, and "above", "below", "within" etc. are understood as including the number itself. If there is a description of "first" or "second", it is only used for the purpose of distinguishing the technical features, and cannot be understood as indicating or implying the relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.

[0035] In the description of the present invention, unless otherwise clearly defined, terms such as setting, installing, connecting, etc. should be understood in a broad sense, and technicians in the relevant technical field can reasonably determine the specific meanings of the above terms in the present invention based on the specific content of the technical solution.

[0036] Reference Figures 1 to 3 In the first aspect of the present invention, a transparent component is used in a lamp and includes a base 100. The base 100 includes a base area 101 and a light-transmitting area 102. The base area 101 is located on both sides of the light-transmitting area 102. It can be understood that the base area 101 is fixedly connected to the light-transmitting area 102, and the base area 101 is a non-light-transmitting material arranged on the periphery of the light-transmitting area 102. The base area 101 is used to fix the transparent component during installation. Further, the base area 101 and the light-transmitting area 102 are made by a two-color molding process. Since the base area 101 is located on the periphery of the light-transmitting area 102, during molding, a two-color molding injection molding machine can be used to first inject a transparent material into the mold, and then the light-transmitting area 102 is molded after the transparent material cools down, and then the non-light-transmitting material is injected to form the base area 101 fixed to the periphery of the light-transmitting area 102 after cooling down.

[0037] It is understandable that the light-transmitting area 102 uses a transparent substrate, a material with high hardness, high transparency and good adhesion, such as polycarbonate (PC) transparent resin. This type of material can provide sufficient hardness to resist scratches and wear during daily use while ensuring transparency. On the other hand, the base area 101 uses a black substrate, a material with high hardness, light shielding and easy molding and bonding with transparent PC material. Polycarbonate (PC) black resin is preferably used. Because the same material has different colors, it can ensure a good bonding with the transparent PC during molding and can also shield the outer edge of the lampshade.

[0038] It is understandable that the light-transmitting area 102 is covered with a hard coating 110, which is mainly based on resin and oil, supplemented by appropriate solvents and additives to form a uniform, transparent coating with a certain hardness and durability. Specifically, resin is the basic skeleton of the hard coating agent. Common resins include alkyd resin, polyurethane resin, epoxy resin, acrylic resin, etc., which have good adhesion, hardness, gloss and chemical resistance; oil is mainly used to increase the flexibility, gloss and anti-aging properties of the coating, such as vegetable oil (tung oil, linseed oil, etc.) and synthetic oil; the role of the solvent is to dilute the resin and oil, so that it is easy to apply and level during construction, and also help to evaporate quickly after film formation, so as to promote the cross-linking and curing of the resin and oil. Commonly used solvents include alcohols, ketones, esters, etc. In order to enhance the specific properties of hard coatings, a series of additives are added, including but not limited to: leveling agent: improve the surface leveling of the coating and reduce the orange peel phenomenon; defoaming agent: prevent and eliminate bubbles generated during the construction process to ensure the flatness of the coating; thickener: adjust the viscosity of the coating to facilitate construction control; anti-settling agent: prevent the sedimentation of pigments and fillers and maintain the stability of the coating; UV absorbers and antioxidants: improve the weather resistance of the coating and delay the aging process.

[0039] Further, the light-transmitting area 102 is provided with a color paint area 103, and the color paint area 103 is coated with an opaque light-shielding layer, and the light-shielding layer includes a primer 111 and a color paint layer 112, and the primer 111 is located between the hard coating layer 110 and the color paint layer 112. It can be understood that the primer 111, as an intermediate layer, can enhance the adhesion between the color paint layer 112 and the hard coating layer 110. Since the hard coating layer 110 usually has a high hardness and chemical stability, the direct coating of the color paint may not achieve the ideal bonding strength. The use of the primer 111 can provide a good bonding platform for the color paint to ensure the overall firmness of the coating. In addition, the primer 111 can provide a smooth transition, so that the color paint layer 112 can be more evenly distributed, improving the smooth effect. Further, in this embodiment, the primer 111 preferably uses an opaque primer 111, which helps to further improve the light-shielding effect.

[0040] Further, the substrate 100 includes a front face 106 and a back face 107. It is understood that a transparent component applied to a lamp, such as a transparent lampshade, has a front face 106 facing the outside of the lamp and a back face 107 facing the light source, and the light shielding layer and the hard coating layer 110 are located on the front face 106. In addition, since the lampshade is often configured to be an outwardly protruding arc, the front face 106 of the substrate 100 is an outwardly protruding arc surface. The light shielding layer and the hard coating layer 110 are coated on the front face 106 of the substrate 100, so that the spraying angle can be conveniently adjusted, and the uneven spraying thickness caused by the concentrated accumulation of the coating can be avoided, which is conducive to improving the uniformity of the spraying, making the coating smooth, and thus improving the visual effect.

[0041] Furthermore, the color paint area 103 has a plurality of hollow portions 105 arranged at intervals, and the hollow portions 105 can transmit light to enhance the aesthetic effect. It is understandable that the hollow portions 105 are not coated with a light shielding layer, and a variety of aesthetic designs can be achieved by setting hollow portions 105 of different shapes. It is understandable that along the width direction of the substrate 100, a plurality of hollow portions 105 are provided, and the hollow portions 105 are arranged in strips, and there is a gap coated with a light shielding layer between two adjacent hollow portions 105.

[0042] Furthermore, the light-transmitting area 102 also includes a transparent area 104 located on one side of the colored paint area 103. The transparent area 104 is coated on the outer periphery of the colored paint area 103. No light-shielding layer is coated on the transparent area 104. While setting the opaque colored paint area 103, the light-transmitting area of ​​the lamp is increased by setting the light-transmitting area 102, thereby ensuring good lighting function while beautifying the appearance.

[0043] Furthermore, a varnish layer 113 is coated on the outer side of the color paint layer 112 away from the substrate 100. It is understood that the varnish layer 113 can significantly improve the glossiness of the surface of the substrate 100 and enhance the visual effect due to its transparent and bright characteristics, and the varnish layer 113 can effectively resist the damage of the color paint layer 112 by the external environment, such as ultraviolet radiation, acid rain, bird droppings, gum and other natural factors, as well as slight scratches and stone strikes, to protect the color paint from being damaged. It is understood that the varnish layer 113 covers the outer wall of the color paint layer 112 and the hollow part 105 at the same time, so as to meet the protection of the color paint layer 112 and the hard coating layer 110.

[0044] In an embodiment of the second aspect of the present invention, a surface coating process is provided for coating a hard coating layer 110, a light shielding layer and a varnish layer 113 on the surface of a substrate 100, comprising the following steps:

[0045] Step 1: Hard coating, apply a hard coating 110 on the surface of the front side 106, adopt a solvent method preparation process, and evenly spray the hard coating material on the surface of the substrate 100 through an automatic coating line. Furthermore, the thickness of the hard coating 110 is controlled between 90μm-180μm, and is mainly cured by ultraviolet (UV) curing. After the spraying is completed, the front side 106 of the substrate 100 is irradiated by an ultraviolet lamp, and the curing temperature is controlled at about 40-60°C, so that the chemical substances in the hard coating 110 react and solidify into a hard paint surface. This curing method has the advantages of fast speed and high hardness, and the hard coating 110 has good wear resistance, UV resistance and transparency, and can protect the substrate 100 from damage by the external environment.

[0046] Step 2: Masking, paste masking paper on the transparent area 104 of the front 106, and paste masking film on the back 107 and the base area 101. It can be understood that this step is used to mask the transparent area 104, so as to leave the color paint area 103, to prevent the color paint from contaminating the transparent area 104 during spraying, and affecting the transmittance of the transparent area 104. It should be noted that the masking paper is a material that has been treated with anti-static, which can effectively prevent the adsorption of dust and the falling of paper fibers, avoid the generation of impurities during spraying, and the paper base is tight, which can effectively prevent paint penetration, and at the same time has high temperature resistance, ensuring that it will not burn when baked in the paint room. The masking film is generally a film made of polyethylene, polypropylene and other materials. Its width is wider than the masking paper, which is more suitable for large-area masking and can withstand high-temperature baking at 60 to 80 degrees.

[0047] In this embodiment, a dual combination method of affixing masking paper to the front side 106 and masking film to the back side 107 and the base area 101 is adopted. Since the colored paint area 103 of the front side 106 has an irregular contour, the operation of attaching the masking paper is relatively convenient and has a certain fault tolerance rate, so the qualified rate of attachment is high; at the same time, the attachment to the back side 107 only needs to prevent the colored paint from entering the substrate 100, and there is no strict area restriction. It only needs to be attached along the outer boundary of the substrate 100. Therefore, the use of masking film for attachment has lower cost.

[0048] Step 3: Primer coating, spraying the primer 111 on the front 106 covered with the hard coating 110 to improve the bonding force between the color paint layer 112 and the hard coating 110. In this process, the primer is sprayed with a high-pressure spray gun through an automatic coating line. During spraying, the surface angle between the spray gun and the front 106 is controlled between 45° and 90°, which helps to reduce the rebound of paint mist, which means that the risk of inhaling paint mist is reduced for the operator, and the chance of pollution of the surrounding environment and unpainted areas is also reduced; it can optimize the coating distribution, and the primer can be more evenly distributed on the surface; and this angle can make the paint particles spread in a wider fan-shaped mode, which helps to make the coating smooth and uniform, and reduce sagging and accumulation. Further, the use of a reasonable angle can improve the efficiency of the coating and reduce the waste of the coating, because the coating has a wider coverage at this angle, reducing the need for overlapping spraying; when the surface angle between the spray gun and the front 106 is controlled between 45° and 90°, it can reduce surface defects and help avoid defects such as orange peel and sagging on the coating surface.

[0049] In this embodiment, the spraying distance of the primer is controlled between 100 mm and 300 mm, which can form a good thickness of the base coating 111. It can be understood that when the spraying distance is less than 100 mm, the spraying distance is too small, which can easily make the base coating 111 too thick, and while consuming more materials, it is easy to have defects such as orange peel and sagging; when the spraying distance is greater than 300 mm, the spraying distance is too large, which can easily lead to the base coating 111 being too thin, and cannot meet the requirements of improving the bonding strength between the color paint layer 112 and the hard coating layer 110.

[0050] Furthermore, the spraying speed is controlled between 25 and 55 square meters per hour, and the spraying pressure is controlled between 0.6 and 2.0 MPa, which can ensure that the primer has enough time to be well atomized and evenly distributed, reduce particles, streaks and sagging in the coating, thereby improving the smoothness and uniformity of the coating; and form a denser and continuous primer layer 111 on the surface of the substrate 100, thereby enhancing the adhesion and durability of the primer layer 111.

[0051] Step 4: Color paint coating, spraying a color paint layer 112 on the front side 106 covered with the primer layer 111. Specifically, the front side 106 of the substrate 100 is now surface treated to ensure that the surface is clean, smooth, and dust-free, and to remove stains such as paint and grease to improve the adhesion of the coating. Furthermore, an automatic line robot is used for spraying to ensure that the color paint coating is uniform and smooth, and the painting and baking are carried out according to the 2B1C process with a line speed of 30-120 meters per minute, and the curing is carried out at a baking temperature of 80°C and a baking time of 30 minutes. It can be understood that the use of a robot improves efficiency and accuracy, ensures that the coating thickness of each part is uniform, avoids errors caused by human operation, thereby improving the consistency and quality stability of the product; and can improve environmental protection and safety. The robot spraying system can effectively reduce paint waste and reduce VOC emissions.

[0052] Step 5: laser engraving, laser engraving the light shielding layer and engraving a hollow portion 105 in the light shielding layer, that is, removing a portion of the color paint layer 112 and the base coat layer 111 by laser engraving, and carving the outline of the hollow portion 105 from the color paint area 103. In addition, after the laser engraving process is completed, the surface is cleaned to remove residual paint and debris to avoid affecting the subsequent coating qualification rate.

[0053] Step 6: Varnish coating, spray a varnish layer 113 on the front side 106 of the substrate 100, so as to cover the color paint area 103, the hollow part 105, and the transparent area 104 with a layer of varnish layer 113 to improve the protective effect. It is understandable that before the varnish coating, the surface of the front side 106 is cleaned by wiping, dust removal, degreasing, etc. to ensure that the surface is smooth, dust-free, and oil-free, so as to improve the adhesion between the coating and the surface of the object. In this step, an automatic line manipulator is used to spray the varnish coating to ensure that the varnish layer 113 is uniform and smooth, and the 1B1C process with a line speed of 30-120 meters / minute is used for spraying and baking. The curing is carried out at a baking temperature of 80°C and a baking time of 40 minutes to accelerate the cross-linking reaction between the varnish molecules and form a hard, bright, and weather-resistant surface coating.

[0054] It can be understood that after the laser engraving process is completed, a layer of hard coating 110 remains in the area of ​​the hollow portion 105 on the surface of the front side 106. In the varnish coating step, the varnish layer 113 located in the area of ​​the hollow portion 105 covers the hard coating 110. Since the varnish layer 113 is directly sprayed on the surface of the substrate 100 of the PU material, the varnish layer 113 has insufficient adhesion and is prone to cracking. Therefore, in the laser engraving process, only the color paint layer 112 and the primer layer 111 need to be removed, which is beneficial to improve the spraying effect of the varnish layer 113 and improve the protective effect of the varnish layer 113 on the color paint layer 112 and the substrate 100.

[0055] Furthermore, after baking, the substrate 100 is cooled and then subjected to a testing process, including hardness and adhesion testing, including the hardness reaching the pencil hardness HB level, the adhesion 100-grid test being OK, and the wear resistance being 1500 cycles without damage, etc., to ensure that the coating quality of each product meets the standards.

[0056] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A transparent component used in a lamp, characterized in that: include: The substrate includes a base area and a light-transmitting area, the base area is located on both sides of the light-transmitting area, the light-transmitting area is covered with a hard coating layer, the light-transmitting area is provided with a colored paint area, the colored paint area is coated with an opaque shading layer, the shading layer includes a primer layer and a colored paint layer, the primer layer is located between the hard coating layer and the colored paint layer, the colored paint area has a plurality of hollow portions arranged at intervals, and the hollow portions can transmit light.

2. A transparent component according to claim 1, characterized in that: The light-transmitting area also includes a transparent area located on one side of the color paint area, and the transparent area is coated on the periphery of the color paint area.

3. A transparent component according to claim 1, characterized in that: A clear varnish layer is applied on the outer side of the color varnish layer away from the substrate.

4. A transparent component according to claim 1, characterized in that: The substrate comprises a front side and a back side, and the light shielding layer and the hard coating layer are located on the front side.

5. A transparent component according to claim 1, characterized in that: The hard coating layer has a thickness of 90 μm-180 μm.

6. Surface coating process, characterized in that: A transparent component applied to any one of claims 1 to 5, comprising a substrate, the substrate having a front side and a back side, the front side having a color paint area and a transparent area, the surface of the color paint area being covered with a hard coating, a primer, a color paint layer and a clear varnish layer, the color paint area having a hollow portion, comprising the following steps: Step 1: hard coating, coating the hard coating on the surface of the front side; Step 2: Masking, pasting masking paper on the transparent area of ​​the front side, and pasting masking film on the back side and the base area; Step 3: Primer coating, spraying the primer on the front surface covered with the hard coating to improve the bonding force between the color paint layer and the hard coating; Step 4: Color paint coating, spraying the color paint layer on the front surface covered with the base coat; Step 5: laser engraving, laser engraving the color paint layer, and engraving the hollow part in the light shielding layer; Step 6: Varnish coating, spraying the varnish layer on the front side of the substrate.

7. The surface coating process according to claim 6, characterized in that: After the hard coating is applied, the hard coating layer is cured by irradiating the hard coating layer with ultraviolet light at a temperature of 40° C. to 60° C.

8. The surface coating process according to claim 6, characterized in that: The base coating is sprayed with a spray gun, and the angle between the spray gun and the front surface during spraying is 45°-90°.

9. The surface coating process according to claim 6, characterized in that: The spraying speed of the primer coating ranges from 25 square meters to 55 square meters per hour, and the spraying pressure is controlled between 0.6 MPa and 2.0 MPa.

10. The surface coating process according to claim 6, characterized in that: In the paint coating, a robot is used for automatic spraying, wherein the line speed during the spraying process is 30 meters to 120 meters per minute, and baking and curing are required after the spraying is completed, the curing temperature is at least 80° C., and the baking time is at least 30 minutes.