Film preparation method for improving PVD binding force of glass
By depositing a metal oxide layer and a metal transition layer on the surface of a glass substrate, and combining the lattice similarity between the metal oxide layer and the glass with the bonding of the transition layer, the problem of poor adhesion between elemental metals and glass is solved, thereby improving the adhesion and allowing for adjustable color appearance.
Patent Information
- Application Number
- CN202411073417.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-05
AI Technical Summary
In traditional coating methods, the lattice constants between elemental metals and glass substrates differ significantly, resulting in poor adhesion between the conductive film and the substrate.
A metal oxide layer is deposited on the surface of a glass substrate, followed by a metal transition layer and a multi-component gradient color appearance layer. The bonding strength is improved by the similarity of the lattice constant between the metal oxide layer and the glass substrate and the bonding of the metal transition layer. Residual stress and thermal stress are reduced by controlling the composition gradient.
It significantly improves the adhesion of glass coatings while maintaining the adjustability of film color appearance, reducing crack driving force and stress singularity, and enhancing connection strength.
Smart Images

Figure CN118895485A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of PVD coating, and in particular relates to a method for preparing a thin film that improves the bonding strength of glass PVD. Background Art
[0002] Smart wearable devices refer to smart terminals that are directly worn by people and embed technologies such as sensors, wireless communications, and multimedia. Based on the natural capabilities of the human body or the environment, they achieve corresponding intelligent information interaction through built-in sensors and integrated chips. At present, smart wearable devices are penetrating into all aspects of daily life. As a link between human-computer interaction, they focus more on solving practical problems in consumers' lives and provide intelligent assistance in people's daily food, clothing, housing, transportation, and health management.
[0003] As people pay more and more attention to health management, the application of bio-monitoring technology in smart wearable devices is becoming more and more common. ECG is a bio-monitoring technology used in mainstream health management products on the market. Apple Watch's definition of ECG: ECG (Electrocardiogram) is an experiment used to record the time nodes and intensity of the sequence of electrical signals that trigger the heartbeat. By analyzing ECG images, doctors can better diagnose whether our heart rate is normal and whether there are problems with heart function. By placing multiple electrodes on the skin to capture electrical pulses in the heart, users only need to open the heart rate measurement app and place their fingers on the digital crown. The app can analyze these pulses to find out whether the user's heart rate is normal. The electrodes placed on the skin generally need to be plated with a conductive film on the glass surface.
[0004] The traditional coating method uses a single metal as a base layer, which is directly attached to a glass substrate, and then a conductive film surface layer is plated on the base layer. Due to the large difference in lattice constants between the single metal and the glass substrate, the film-base bonding strength of the entire conductive film is poor. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a method for preparing a thin film that improves the bonding strength of glass PVD, by coating a metal oxide layer on the surface of a glass substrate, and then coating a metal transition layer and a multi-component gradient color appearance layer, thereby significantly improving the bonding strength of the glass coating without reducing the adjustability of the final film color appearance.
[0006] To achieve the above object, the technical solution of the present invention is as follows:
[0007] The present invention provides a method for preparing a thin film for improving the glass PVD bonding strength, comprising the steps of:
[0008] S1: After cleaning and drying the glass substrate, fix it in the vacuum chamber of the coating machine, and heat and evacuate the vacuum chamber;
[0009] S2: After the background vacuum of the vacuum chamber reaches 0.005Pa, argon gas is introduced to make the gas pressure in the furnace reach a specific value;
[0010] S3: Start the ion source, switch to constant pressure mode, and clean the glass substrate by ion bombardment;
[0011] S4: turn off the ion source, introduce oxygen to raise the gas pressure in the furnace to a specific value, turn on the bias power supply, set the duty cycle; turn on a pair of titanium targets to deposit a titanium oxide layer;
[0012] S5: turn off the oxygen, adjust the titanium target current, perform sputtering, remove titanium oxide on the target surface and deposit a pure titanium layer;
[0013] S6: turn off oxygen, turn on another pair of titanium targets, turn on the silicon target, introduce acetylene, and deposit a TiSiC film layer;
[0014] S7: close a pair of titanium targets, adjust the silicon target current, turn on nitrogen, adjust the acetylene flow rate, and deposit a TiSiCN film layer;
[0015] S8: Turn off all target power supplies, bias power supplies, and gases to end the coating.
[0016] Furthermore, in the thin film preparation method, the target material is configured with: two pairs of titanium targets, one pair of silicon targets, and an anode layer ion source; wherein the anode layer ion source is installed on the furnace door. The anode layer ion source is used to clean and activate the surface of the substrate before coating, and is installed on the furnace door to prevent the ion beam from affecting the target material.
[0017] Furthermore, the cleaning method in step S1 is ultrasonic cleaning, and the drying method is vacuum drying.
[0018] Furthermore, in step S1, the vacuum chamber is heated and then kept at 100°C.
[0019] Furthermore, in step S2, the specific value of the gas pressure in the furnace is 0.3Pa.
[0020] Furthermore, in step S3, the voltage of the constant voltage mode is set to 800-1000 V, and the ion bombardment time is 10 minutes.
[0021] Furthermore, in step S4, the specific value of the gas pressure in the furnace is 0.5Pa, the voltage of the bias power supply is set to 80V, the duty cycle is set to 50%, the titanium target current is set to 10-13A, and the deposition time of the titanium oxide layer is 8 minutes. In the present application, more oxygen is introduced to make the gas pressure in the furnace reach 0.5Pa, which can increase the proportion of chromium oxide in the film and reduce the proportion of pure chromium; considering that the glass substrate is not conductive, the bias voltage is set to 80V, which can avoid the glass substrate from igniting under the premise of ensuring sufficient bias voltage.
[0022] Furthermore, in step S5, the titanium target current is adjusted from 10-13A to 13-15A, and the sputtering time is 20 minutes.
[0023] Furthermore, in step S6, the current of another pair of titanium targets is set to 13-15A, the current of the silicon target is set to 10-13A, the initial acetylene flow rate is set to 30-40sccm, and the acetylene flow rate is stepped to 80-90sccm at a rate of 0.5sccm / min, and the TiSiC film layer is deposited for 100 minutes.
[0024] Further, in step S7, the silicon target current is adjusted to 15-18A, the initial nitrogen flow rate is set to 10-20sccm, the nitrogen flow rate is increased to 40-50sccm at a rate of 0.5sccm / min, and the acetylene flow rate is increased to 95-105sccm at a rate of 0.25sccm / min, and then the TiSiCN film layer is deposited for 60 minutes.
[0025] Furthermore, in steps S4-S7, the titanium target may be replaced by a chromium target, a chromium oxide layer is deposited in step S4, a pure chromium layer is deposited in step S5, a CrSiC layer is deposited in step S6, and a CrSiCN layer is deposited in step S7.
[0026] Compared with the prior art, the present invention has the following beneficial effects: by first plating a metal oxide layer on the surface of a glass substrate, and then plating a pure metal transition layer, the metal oxide layer and the glass substrate are both oxides, and the lattice constant of the metal oxide layer and the glass are similar, so the bonding force between the two is strong, and the metal transition layer and the metal oxide layer are strongly bonded through the bonding between the same metal atoms, thereby improving the bonding force between the single metal and the glass. Finally, plating multiple gradient color appearance layers can significantly improve the bonding force of the glass coating without reducing the adjustability of the final film color appearance. By controlling the composition gradient from the single metal to the multi-element color appearance layer, the residual stress and thermal stress can be reduced, the stress singularity of the interface intersection and the stress free end point in the connecting material can be eliminated, the connection strength can be enhanced, and the crack driving force can also be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1It is a flowchart of the preparation method of this embodiment.
[0028] Figure 2 Schematic diagram of the membrane structure of this embodiment. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0030] To achieve the above object, the technical solution of the present invention is as follows:
[0031] See also Figure 1 As shown, this embodiment provides a method for preparing a thin film with improved glass PVD bonding strength, wherein the target material configuration includes two pairs of titanium targets, one pair of silicon targets, and an anode layer ion source; wherein the anode layer ion source is installed on the furnace door, and the coating method includes the following steps:
[0032] S1: After cleaning and drying the glass substrate, fix it in the vacuum chamber of the coating machine, and heat and evacuate the vacuum chamber;
[0033] S2: After the background vacuum of the vacuum chamber reaches 0.005Pa, argon gas is introduced to make the gas pressure in the furnace reach a specific value;
[0034] S3: Start the ion source, switch to constant pressure mode, and clean the glass substrate by ion bombardment;
[0035] S4: turn off the ion source, introduce oxygen to raise the gas pressure in the furnace to a specific value, turn on the bias power supply, set the duty cycle; turn on a pair of titanium targets to deposit a titanium oxide layer;
[0036] S5: turn off the oxygen, adjust the titanium target current, perform sputtering, remove titanium oxide on the target surface and deposit a pure titanium layer;
[0037] S6: turn off oxygen, turn on another pair of titanium targets, turn on the silicon target, introduce acetylene, and deposit a TiSiC film layer;
[0038] S7: close a pair of titanium targets, adjust the silicon target current, turn on nitrogen, adjust the acetylene flow rate, and deposit a TiSiCN film layer;
[0039] S8: Turn off all target power supplies, bias power supplies, and gases to end the coating.
[0040] Furthermore, in the thin film preparation method, the anode layer ion source is used to clean and activate the substrate surface before coating, and is installed on the furnace door to prevent the ion beam from affecting the target material.
[0041] Furthermore, the cleaning method in step S1 is ultrasonic cleaning, and the drying method is vacuum drying.
[0042] Furthermore, in step S1, the vacuum chamber is heated and then kept at 100°C.
[0043] Furthermore, in step S2, the specific value of the gas pressure in the furnace is 0.3Pa.
[0044] Furthermore, in step S3, the voltage of the constant voltage mode is set to 800-1000 V, and the ion bombardment time is 10 minutes.
[0045] Furthermore, in step S4, the specific value of the gas pressure in the furnace is 0.5Pa, the voltage of the bias power supply is set to 80V, the duty cycle is set to 50%, the titanium target current is set to 10-13A, and the deposition time of the titanium oxide layer is 8 minutes. In the present application, more oxygen is introduced to make the gas pressure in the furnace reach 0.5Pa, which can increase the proportion of chromium oxide in the film and reduce the proportion of pure chromium; considering that the glass substrate is not conductive, the bias voltage is set to 80V, which can avoid the glass substrate from igniting under the premise of ensuring sufficient bias voltage.
[0046] Furthermore, in step S5, the titanium target current is adjusted from 10-13A to 13-15A, and the sputtering time is 20 minutes.
[0047] Furthermore, in step S6, the current of another pair of titanium targets is set to 13-15A, the current of the silicon target is set to 10-13A, the initial acetylene flow rate is set to 30-40sccm, and the acetylene flow rate is stepped to 80-90sccm at a rate of 0.5sccm / min, and the TiSiC film layer is deposited for 100 minutes.
[0048] Further, in step S7, the silicon target current is adjusted to 15-18A, the initial nitrogen flow rate is set to 10-20sccm, the nitrogen flow rate is increased to 40-50sccm at a rate of 0.5sccm / min, and the acetylene flow rate is increased to 95-105sccm at a rate of 0.25sccm / min, and then the TiSiCN film layer is deposited for 60 minutes.
[0049] See also Figure 2, the metal Me in the figure is metal Ti. Compared with the prior art, the beneficial effect of this embodiment is: by first plating a metal oxide layer on the surface of the glass substrate, and then plating a pure metal transition layer, the metal oxide layer and the glass substrate are both oxides, and the lattice constant of the metal oxide layer and the glass are similar, and the bonding force between the two is strong, and the metal transition layer and the metal oxide layer are strongly bonded through the bonding between the same metal atoms, thereby improving the bonding force between the single metal and the glass. Finally, multiple gradient color appearance layers are plated, which can significantly improve the bonding force of the glass coating without reducing the adjustability of the final film color appearance. By controlling the composition gradient from the single metal to the multi-element color appearance layer, the residual stress and thermal stress can be reduced, and the stress singularity of the interface intersection and the stress free end point in the connecting material can be eliminated. The connection strength can also be enhanced and the crack driving force can be reduced.
[0050] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a thin film for improving the bonding strength of glass PVD, It is characterized in that Includes steps: S1: After cleaning and drying the glass substrate, fix it in the vacuum chamber of the coating machine, and heat and evacuate the vacuum chamber; S2: After the background vacuum of the vacuum chamber reaches 0.005Pa, argon gas is introduced to make the gas pressure in the furnace reach a specific value; S3: Start the ion source, switch to constant pressure mode, and clean the glass substrate by ion bombardment; S4: turn off the ion source, introduce oxygen to raise the gas pressure in the furnace to a specific value, turn on the bias power supply, set the duty cycle; turn on a pair of titanium targets to deposit a titanium oxide layer; S5: turn off the oxygen, adjust the titanium target current, perform sputtering, remove titanium oxide on the target surface and deposit a pure titanium layer; S6: turn off oxygen, turn on another pair of titanium targets, turn on the silicon target, introduce acetylene, and deposit a TiSiC film layer; S7: close a pair of titanium targets, adjust the silicon target current, turn on nitrogen, adjust the acetylene flow rate, and deposit a TiSiCN film layer; S8: Turn off all target power supplies, bias power supplies, and gases to end the coating.
2. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In the method, the target material configuration includes: two pairs of titanium targets, one pair of silicon targets, and an anode layer ion source; wherein the anode layer ion source is installed on the furnace door.
3. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S1, the vacuum chamber is heated and then kept at 100°C.
4. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S2, the specific value of the gas pressure in the furnace is 0.3Pa.
5. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S3, the voltage of the constant voltage mode is set to 800-1000 V, and the ion bombardment time is 10 minutes.
6. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S4, the specific value of the gas pressure in the furnace is 0.5 Pa, the voltage of the bias power supply is set to 80 V, the duty cycle is set to 50%, the titanium target current is set to 10-13 A, and the deposition time of the titanium oxide layer is 8 minutes.
7. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S5, the titanium target current is adjusted from 10-13 A to 13-15 A, and the sputtering time is 20 minutes.
8. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S6, the current of another pair of titanium targets is set to 13-15A, the current of the silicon target is set to 10-13A, the initial acetylene flow rate is set to 30-40sccm, and the acetylene flow rate is stepped to 80-90sccm at a rate of 0.5sccm / min, and the TiSiC film layer is deposited for 100 minutes.
9. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In step S7, the silicon target current is adjusted to 15-18A, the initial nitrogen flow rate is set to 10-20sccm, the nitrogen flow rate is increased to 40-50sccm at a rate of 0.5sccm / min, and the acetylene flow rate is increased to 95-105sccm at a rate of 0.25sccm / min, and then the TiSiCN film is deposited for 60 minutes.
10. A method for preparing a thin film for improving glass PVD bonding strength as claimed in claim 1, It is characterized in that In steps S4-S7, the titanium target is replaced by a chromium target, a chromium oxide layer is deposited in step S4, a pure chromium layer is deposited in step S5, a CrSiC layer is deposited in step S6, and a CrSiCN layer is deposited in step S7.
Citation Information
Cited By
Film coating method for metal decorating part
CN120505595A
A coating method for metal decorative parts
CN120505595B