Multi-element alloy electrode for hydrogen production by alkaline electrolysis of water and preparation method of multi-element alloy electrode

By using double-sided coating technology of multi-alloys such as cobalt, nickel, chromium, tungsten, molybdenum and aluminum powder in alkaline electrolytic hydrogen production technology, the problems of instability and high cost of electrode materials in high temperature environments are solved. , realizes the efficient potential reduction and prolonging of the electrode, and is suitable for large-scale production.

CN118895531APending Publication Date: 2024-11-05BEIJING HUAYI HYDROGEN TECH CO LTD
View PDF 0 Cites 7 Cited by

Patent Information

Application Number
CN202411029412.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

In the existing alkaline electrolytic hydrogen production technology, the electrode materials are unstable in high temperature environments, the catalyst costs are high, and the component ratio is unclear, resulting in low efficiency and short life, making it difficult to adapt to large-scale production.

Method used

Aerosolized preparation is made by cobalt, nickel, chromium, tungsten, molybdenum and other multi-alloy powders and aluminum powders. The mixture of ultrafine multi-alloy powder and Rainey nickel powder is sprayed on the nickel grid electrode through double-sided coating technology. , combined with plasma spraying technology, improve the high temperature resistance and catalytic effect of the electrode.

Benefits of technology

Effectively reduce the electrode potential at high temperatures, improve the stability and life of the electrode, is suitable for large-scale production, and significantly improves the efficiency of hydrogen production by alkaline electrolysis water.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118895531A_ABST
    Figure CN118895531A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-element alloy electrode for hydrogen production through alkaline electrolysis of water and a preparation method of the multi-element alloy electrode, and relates to the technical field of hydrogen production electrodes. The preparation method comprises the following steps that firstly, cobalt 42, nickel 25, chromium 21, tungsten 7 and molybdenum 5 are fully mixed and then smelted, and spherical multi-element alloy powder is prepared in a gas atomization mode; secondly, spherical multi-element alloy powder with the particle size being 25-45 micrometers is fully mixed with spherical aluminum powder; and thirdly, the spherical multi-element alloy powder with the particle size larger than 45 micrometers is subjected to ball milling and crushing. The catalyst of the electrode is prepared from the cobalt-based multi-component alloy material, has a more reasonable electrode structure, can effectively reduce the electrode potential at high temperature, and is good in stability, long in service life and suitable for large-scale production; and different catalyst coatings are adopted on the two surfaces of the electrode, so that the high-temperature resistance of the electrode can be ensured, and the service life of the electrode is longer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen production electrodes, and in particular relates to a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis and a preparation method thereof. Background Art

[0002] Energy issues have always been a common concern of the world. Renewable energy generation is volatile, and a medium is needed to store the fluctuating renewable energy. Hydrogen energy has both material and energy properties. Renewable energy can convert electrical energy into hydrogen energy for storage and transportation through the electrolysis of water.

[0003] Alkaline water electrolysis is a widely used industrial water electrolysis hydrogen production technology due to its mature technology and relatively low cost. However, the efficiency of alkaline water electrolysis is low, and compared with PEM, AEM and SOEC, the efficiency is far behind. Although alkaline water electrolysis has the advantage of low cost, how to improve the hydrogen production efficiency of alkaline cells is still the research focus of major companies and scientific research institutions. At present, high-temperature alkaline water electrolysis is the most promising hydrogen production technology to improve the efficiency of alkaline electrolyzers. However, high-temperature alkaline water electrolysis is affected by many factors, among which the electrode is one of the influencing factors. Breakthroughs in high-temperature and high-efficiency electrode technology are expected to promote the development of high-temperature alkaline water electrolysis technology, thereby improving the efficiency of alkaline water electrolysis hydrogen production.

[0004] For example, the publication number CN115725982A discloses an industrial method for preparing a bifunctional electrode, a bifunctional electrode and its application, the core idea of ​​which is "using a high-temperature plasma spraying method to spray alloy powder on an electrode substrate, the alloy powder mainly comprising 70wt%-80wt% Ni, 10wt%-20wt% Al, and 3wt%-8wt% Fe." This scheme uses the same alloy powder to prepare the cathode and anode, and there is no need to spray the cathode alloy powder and the anode alloy powder separately, which saves materials and simplifies the preparation process.

[0005] For example, the publication number CN116288509A is a cathode for alkaline water electrolysis to produce hydrogen, and its preparation method and application. Its core idea is "mixing nickel powder, aluminum powder, platinum group metal powder and graphene powder to obtain mixed metal powder; using plasma spraying to spray the mixed metal powder onto the surface of the electrode substrate to form a coating, and obtain a hydrogen evolution electrode." This scheme uses plasma spraying to melt platinum group metals and graphene with nickel and aluminum at high temperature and then spray them onto the surface of the electrode substrate to form a coating. Not only does the coating have better bonding with the substrate, the coating is more uniform, the service life of the electrode is improved, and the hydrogen evolution potential is lower.

[0006] For example, the preparation method of the alkaline water electrolysis hydrogen production multi-catalyst and nickel wire mesh electrode with publication number CN117344334A has the core idea that "the catalyst includes the mass percentage of: Ni: 40-80%; and also includes one or more of Fe, Co, Mo, and W. In the catalyst, Fe, Co, Mo, and W are one or more of the following mass percentages: Fe: 5-40%; Co: 5-40%; Mo: 5-40%; W: 5-40%". This scheme can improve the conductivity and reaction activity of the catalyst by adding elements such as Fe, Co, W, and Mo to Ni metal, thereby improving the efficiency of the catalyst in producing hydrogen by water electrolysis.

[0007] However, the above existing solutions still have some problems: the publication number is CN115725982A, which is a method for industrially preparing a bifunctional electrode, a bifunctional electrode and its application. The alloy powder process of this solution is too simple, and iron is difficult to stabilize in the harsh environment of an alkaline electrolytic cell and will soon be dissolved, especially in a high-temperature alkaline environment of more than 100 degrees, where it will dissolve faster. This invention will not only cause electrode catalytic failure, but also cause damage to the electrolytic cell and the diaphragm; the publication number is CN116288509A, which is a cathode for alkaline water electrolysis to produce hydrogen, and its preparation method and application. The price of the platinum group metal powder in this solution is very high. It is expensive. The price of platinum is 300 yuan per gram, and not even one gram of platinum can be used in one kilogram of catalyst powder. This powder material is not very reasonable and is not suitable for promotion. Moreover, this solution only helps the potential of the electrode to a certain extent. The service life will be sharply shortened under high temperature environment and cannot improve the efficiency of the alkaline electrolyzer; the preparation method of the multi-catalyst and nickel wire mesh electrode for hydrogen production by alkaline electrolysis of water with publication number CN117344334A, the alloy powder material in this solution adopts a multi-alloy method. In theory, the catalytic effect of the catalyst will be very good, but the component ratio in the alloy powder is unclear, and it contains a large amount of iron, which cannot be applied to high-temperature alkaline environment.

[0008] Based on this, a multi-element alloy electrode for hydrogen production by alkaline water electrolysis and a preparation method thereof are proposed, thereby providing a multi-element alloy electrode for hydrogen production by alkaline water electrolysis that can not only effectively reduce the electrode potential at high temperature, but also has good stability and long life and is suitable for large-scale production. Summary of the invention

[0009] The object of the present invention is to provide a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0010] In order to solve the above technical problems, the present invention is achieved through the following technical solutions:

[0011] The present invention is a method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis, comprising the following steps:

[0012] Step 1: 42 parts of cobalt, 25 parts of nickel, 21 parts of chromium, 7 parts of tungsten and 5 parts of molybdenum are fully mixed and smelted, and spherical multi-element alloy powder is prepared by gas atomization;

[0013] Step 2: Fully mix spherical multi-element alloy powder with a particle size of 25 to 45 microns and spherical aluminum powder;

[0014] Step 3: ball-milling the spherical multi-element alloy powder with a particle size greater than 45 microns to form an ultrafine crushed multi-element alloy powder with a particle size less than 25 microns, and mixing it with the ultrafine spherical multi-element alloy powder with a particle size less than 25 microns produced by atomization to form an ultrafine multi-element alloy powder with a particle size less than 25 microns, and then mixing the ultrafine multi-element alloy powder with Raney nickel powder;

[0015] Step 4: The nickel mesh electrode adopts double-sided coating technology, and the nickel mesh is sandblasted on both sides before spraying. After the sandblasting is completed, the spherical multi-element alloy powder mixed with the spherical aluminum powder in the step 2 is sprayed onto one side of the nickel mesh by plasma spraying technology, and the coating thickness is 60 to 100 microns;

[0016] Step 5: then turn the nickel mesh over, and use plasma spraying technology to spray the ultrafine multi-element alloy powder mixed in step 3 and the Raney nickel mixed powder onto the other side of the nickel mesh, with a coating thickness of 60 to 100 microns;

[0017] Step 6: Activate the sprayed electrode, clean it and then put it into the electrolytic cell for use.

[0018] Furthermore, in the step 2, the mass ratio of the spherical multi-element alloy powder to the spherical aluminum powder is 8:2.

[0019] Furthermore, in the step 2, the particle size of the spherical aluminum powder is 45 to 90 microns.

[0020] Furthermore, in the step three, the ratio of the ultrafine multi-element alloy powder to the Raney nickel powder is 2:8.

[0021] Furthermore, in the Raney nickel powder, the particle size of the aluminum powder is 45 to 90 microns, the particle size of the nickel powder is 25 to 45 microns, and the ratio of the aluminum powder to the nickel powder is 2:8.

[0022] Furthermore, the activation of the sprayed electrode in step 6 includes the following steps:

[0023] Place the sprayed electrode into a 30% potassium hydroxide solution at 80 degrees Celsius for 3 to 5 hours of activation.

[0024] The present invention has the following beneficial effects:

[0025] 1. The catalyst of the electrode of the present invention is made of cobalt-based multi-element alloy material, which has a more reasonable electrode structure, can effectively reduce the electrode potential at high temperature, and has good stability and long life, and is suitable for large-scale production;

[0026] 2. The electrode of the present invention adopts different catalyst coatings on both sides, which can not only ensure the electrode potential is reduced, have excellent catalytic effect, but also ensure the high temperature resistance of the electrode, making the life of the electrode longer;

[0027] 3. The nickel mesh electrode of the present invention adopts double-sided coating technology. The nickel mesh is sandblasted on both sides before spraying. After the sandblasting is completed, the spherical multi-element alloy powder mixed with spherical aluminum powder is sprayed on one side of the nickel mesh by plasma spraying technology, and the powder mixed with ultrafine multi-element alloy powder and Raney nickel powder is sprayed on the other side of the nickel mesh, thereby having a double-sided protection effect, so that the nickel mesh electrode has a longer life in a high temperature concentrated alkali environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0029] Figure 1 It is a schematic diagram of the preparation process of the present invention;

[0030] Figure 2 It is a schematic diagram of the spherical multi-element alloy powder mixed with spherical aluminum powder and the ultrafine multi-element alloy powder mixed with Raney nickel powder of the present invention;

[0031] Figure 3 It is a schematic diagram of the coating of the present invention before activation;

[0032] Figure 4 It is a schematic diagram of the coating after activation of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Embodiment 1:

[0035] See also Figure 1-4As shown, the present invention is a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis, comprising the following steps:

[0036] Step 1: 42 parts of cobalt, 25 parts of nickel, 21 parts of chromium, 7 parts of tungsten and 5 parts of molybdenum are fully mixed and smelted, and spherical multi-element alloy powder is prepared by gas atomization;

[0037] The spherical multi-element alloy powder of the present invention contains cobalt, nickel, chromium, tungsten and molybdenum. Except for chromium, these materials are all good alkaline electrode catalyst materials. The multi-element alloy interacts with each other to achieve a more efficient alkaline electrode catalytic effect. Moreover, chromium has a strong corrosion resistance. After adding chromium, the corrosion resistance of the coating can be effectively improved, so that the catalyst coating can have a longer life in alkaline solution.

[0038] Step 2: Fully mix the spherical multi-element alloy powder with a particle size of 25 to 45 microns and the spherical aluminum powder with a particle size of 45 to 90 microns, and the mass ratio of the spherical multi-element alloy powder to the spherical aluminum powder is specifically 8:2.

[0039] Step 3: ball mill the spherical multi-element alloy powder with a particle size greater than 45 microns to form an ultrafine crushed multi-element alloy powder with a particle size less than 25 microns, and mix it with the ultrafine spherical multi-element alloy powder with a particle size less than 25 microns produced by atomization to form an ultrafine multi-element alloy powder with a particle size less than 25 microns, and then mix the ultrafine multi-element alloy powder with Raney nickel powder. In this embodiment, the ratio of ultrafine multi-element alloy powder to Raney nickel powder is specifically 2:8, wherein the particle size of aluminum powder in Raney nickel powder is 45-90 microns, the particle size of nickel powder is 25-45 microns, and the ratio of aluminum powder to nickel powder is 2:8.

[0040] Specific as Figure 2 As shown, Figure 2 The left side is a schematic diagram of spherical multi-element alloy powder mixed with spherical aluminum powder. Figure 2 On the middle right is a schematic diagram of ultrafine multi-element alloy powder mixed with Raney nickel powder.

[0041] Step 4: The nickel mesh electrode adopts double-sided coating technology. The nickel mesh is sandblasted on both sides before spraying. After the sandblasting is completed, the spherical multi-element alloy powder mixed with the spherical aluminum powder mixed in the step 2 is sprayed onto one side of the nickel mesh by plasma spraying technology. The coating thickness is 60 to 100 microns. The high temperature resistance is enhanced by mixing the spherical multi-element alloy powder with the spherical aluminum powder coating.

[0042] Step 5: then turn the nickel mesh over, and use plasma spraying technology to spray the ultrafine multi-element alloy powder mixed in the step 3 and the Raney nickel powder mixed on the other side of the nickel mesh, with a coating thickness of 60 to 100 microns. The ultrafine multi-element alloy powder mixed with the Raney nickel powder coating makes the catalytic performance stronger;

[0043] The Raney nickel catalyst coating becomes porous after activation, and the surface of the Raney nickel forms a nanometer surface structure due to ablation, which has a very significant effect on reducing the electrode potential. The electrode catalyst coating of the present invention is improved on the basis of the Raney nickel catalyst coating, so it inherently has the excellent catalytic effect of the Raney nickel catalyst coating.

[0044] The coating formed after double-sided spraying is as follows Figure 3 As shown, the powder particles in a semi-molten state collide with the substrate. After the coating is formed, the spherical powder will become flat, and the coating will be tightly mechanically bonded to the nickel mesh substrate after sandblasting, and there will be local metallurgical bonding. Since aluminum and nickel will undergo a thermite reaction during the heating process, a pit-shaped nano-microstructure will appear on the reaction ablation surface of the two. On the front side, there is a certain amount of nickel in the spherical multi-element alloy powder, which will locally undergo a thermite reaction with aluminum, forming a pit-shaped nano-rough structure on the powder surface. On the back side, the nickel powder and the aluminum powder undergo a thermite reaction, forming a pit-shaped nano-rough structure on the surface. After heating, the spherical ultrafine multi-element alloy powder and the crushed ultrafine multi-element alloy powder are hit on the nickel mesh substrate and the Raney nickel coating to form a flat coating.

[0045] The present invention adopts double-sided coating technology. Although the double-sided coating cannot significantly reduce the potential compared with the single-sided coating, it can reduce it by 30 to 50 millivolts, further reducing the electrode potential; and the double-sided coating has a double-sided protection effect, protecting the pure nickel mesh on both sides, thereby allowing the nickel mesh electrode to have a longer life in a high-temperature concentrated alkali environment.

[0046] The coating thickness adopted by the present invention is relatively thin, which is 1 / 2 to 2 / 3 of the ordinary electrode coating. The thicker the coating thickness is, the worse the bonding strength is. The present invention reduces the coating thickness, further improves the bonding strength of the coating, and increases the life of the coating. The cost of the electrode catalyst is mainly the material cost, and the spraying cost can be ignored. The present invention reduces the coating thickness, which offsets the cost increase caused by double-sided spraying to a certain extent. Under the premise that the cost is not increased much, the electrode potential is reduced, the electrode life is increased, and it can also adapt to high temperature alkaline environment.

[0047] Step 6: Place the sprayed electrode into a 30% potassium hydroxide solution at 80 degrees Celsius for activation for 3 to 5 hours. Finally, clean it and load it into the electrolytic cell for use.

[0048] Among them, the activated electrode catalyst is Figure 4As shown, during the activation process, aluminum will react violently with 30% sodium hydroxide and be dissolved by the sodium hydroxide; the ablation surface formed by the reaction of aluminum and nickel will appear on the surface of the electrode; the ultrafine alloy powder embedded in the aluminum layer will peel off from the electrode due to the dissolution of aluminum; the aluminum mixed in the gaps will become pores after dissolution, forming a porous coating.

[0049] The ultrafine multi-element alloy powder of the present invention has a smaller particle size and melts faster. It can be fully burned in the plasma flame flow and even form a completely liquid state. During the spraying process, the nickel powder is generally in a semi-molten state. If the nickel powder becomes a completely molten state, it will contact and fuse with the surrounding nickel powder to form large particles, seriously affecting the coating quality. The ultrafine multi-element alloy powder has a small content and a small particle size. Even if it is in a completely molten state, the powder will not agglomerate to form large particles. Instead, it can collide and strike with the semi-molten nickel powder, ablate the surface, and form a nano-scale surface roughness structure.

[0050] The current trend of alkaline electrode catalysts is that the finer the powder material, the better the catalytic effect, because powder materials with small particle sizes have a larger specific surface area and can effectively catalyze the electrode. Therefore, the ultrafine multi-element alloy powder material of the present invention has a very obvious improvement in the catalytic effect of the electrode. However, if all powder materials are ultrafine powders, the fluidity of the powder materials will be very poor, and the powder feeder will have great difficulty in feeding the powder. Therefore, the ultrafine multi-element alloy powder material is mixed with the Raney nickel powder material with large particle size and good fluidity. The two can obtain good powder fluidity and the catalytic advantages of the ultrafine multi-element alloy powder under the ratio of the present invention.

[0051] Ultrafine multi-element alloy powder will form coarse powder in the process of powder making. The coarse powder is crushed by ball milling to form ultrafine crushed multi-element alloy powder. The structure of crushed powder is very complex, and there are a lot of nano-rough structures and a lot of catalytic points, which are very helpful in reducing the electrode potential. However, the fluidity of crushed powder is very poor, so the amount mixed into the whole powder is small, adsorbed on Raney nickel, and the fluidity of Raney nickel is used to bring the crushed ultrafine multi-element alloy powder into the plasma flame flow for spraying.

[0052] At the same time, the present invention fully utilizes the powder prepared by aerosolization, ensures that the waste powder rate is 0, and can effectively reduce the powder cost.

[0053] Embodiment 2:

[0054] See also Figure 1-4 As shown, a method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis is described. The specific steps of the preparation method described in this embodiment are as follows:

[0055] Step 1: Preparation of alloy powder: accurately weigh the raw materials according to the ratio of 42% cobalt, 25% nickel, 21% chromium, 7% tungsten and 5% molybdenum, thereby effectively reducing the electrode potential; then use vacuum induction melting technology to ensure the uniformity of the alloy composition, and then use the gas atomization process to prepare spherical multi-element alloy powder with an average particle size of 35 microns.

[0056] Step 2: Preparation of mixed powder: Select spherical aluminum powder with a particle size of 30 microns (20% by mass) and mix it thoroughly with the spherical multi-element alloy powder (80% by mass) prepared in step 1 to ensure uniform mixing to improve the conductivity and corrosion resistance of the coating.

[0057] Step 3: Mixing ultrafine powder with Raney nickel: Ball-mill the spherical multi-element alloy powder with a particle size greater than 45 microns to an average particle size of 15 microns, and mix it with the fine powder (<25 microns) produced during the atomization process to form an ultrafine multi-element alloy powder. Subsequently, the ultrafine multi-element alloy powder is mixed at a ratio of 20% and Raney nickel powder 80%, wherein the aluminum powder particle size is 60 microns, the nickel powder particle size is 35 microns, and the ratio of aluminum powder to nickel powder is 2:8, in order to enhance the catalytic activity and durability of the electrode.

[0058] Step 4: Double-sided coating spraying: Sandblast the nickel mesh on both sides to enhance the adhesion of the coating. First, spray the powder mixed in step 2 on one side of the nickel mesh, and the coating thickness is controlled at 80 microns to ensure good conductivity and corrosion resistance. Then turn the nickel mesh over and spray the ultrafine powder mixed in step 3 on the other side, and the coating thickness is also 80 microns to optimize the electrolysis efficiency. By using double-sided coating technology, the potential of the electrode is further reduced, and the electrode can be further protected from high temperatures.

[0059] In other embodiments, HS188 with a particle size of 25 to 45 microns mixed with aluminum powder may be used as a catalyst, HS6B ultrafine powder mixed with Raney nickel powder may be used as a catalyst, and a stainless steel mesh may be used instead of a nickel mesh as a substrate.

[0060] Step 5: Activation and cleaning: Place the sprayed electrode in a 30% potassium hydroxide solution at 80°C for 4 hours to ensure that a stable catalytic layer is formed on the electrode surface. Then thoroughly clean the electrode to remove residues and prepare to load it into the electrolytic cell.

[0061] Thereby significantly improving the efficiency of hydrogen production by water electrolysis and effectively improving the durability and stability of the electrode under long-term use.

[0062] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0063] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the present invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis, characterized in that: The following steps are involved: Step 1: 42 parts of cobalt, 25 parts of nickel, 21 parts of chromium, 7 parts of tungsten and 5 parts of molybdenum are fully mixed and smelted, and spherical multi-element alloy powder is prepared by gas atomization; Step 2: Fully mix spherical multi-element alloy powder with a particle size of 25 to 45 microns and spherical aluminum powder; Step 3: ball-milling the spherical multi-element alloy powder with a particle size greater than 45 microns to form an ultrafine crushed multi-element alloy powder with a particle size less than 25 microns, and mixing it with the ultrafine spherical multi-element alloy powder with a particle size less than 25 microns produced by atomization to form an ultrafine multi-element alloy powder with a particle size less than 25 microns, and then mixing the ultrafine multi-element alloy powder with Raney nickel powder; Step 4: The nickel mesh electrode adopts double-sided coating technology, and the nickel mesh is sandblasted on both sides before spraying. After the sandblasting is completed, the spherical multi-element alloy powder mixed with the spherical aluminum powder in the step 2 is sprayed onto one side of the nickel mesh by plasma spraying technology, and the coating thickness is 60 to 100 microns; Step 5: then turn the nickel mesh over, and use plasma spraying technology to spray the ultrafine multi-element alloy powder mixed in step 3 and the Raney nickel mixed powder onto the other side of the nickel mesh, with a coating thickness of 60 to 100 microns; Step 6: Activate the sprayed electrode, clean it and then put it into the electrolytic cell for use.

2. The method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: In the step 2, the mass ratio of the spherical multi-element alloy powder to the spherical aluminum powder is 8:

2.

3. The method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis according to claim 2, characterized in that: The particle size of the spherical aluminum powder in step 2 is 45 to 90 microns.

4. The method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: In the step three, the ratio of the ultrafine multi-element alloy powder to the Raney nickel powder is 2:

8.

5. The method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis according to claim 4, characterized in that: The particle size of the aluminum powder in the Raney nickel powder is 45 to 90 microns, the particle size of the nickel powder is 25 to 45 microns, and the ratio of the aluminum powder to the nickel powder is 2:

8.

6. The method for preparing a multi-element alloy electrode for producing hydrogen by alkaline water electrolysis according to claim 1, characterized in that: The step 6 of activating the sprayed electrode comprises the following steps: Place the sprayed electrode into a 30% potassium hydroxide solution at 80 degrees Celsius for 3 to 5 hours of activation.

7. A multi-element alloy electrode for producing hydrogen by alkaline water electrolysis, characterized in that: The multi-element alloy electrode for producing hydrogen by alkaline water electrolysis is prepared according to the preparation method described in any one of claims 1 to 6.

Citation Information

Cited By

  • Double-sided different-coating electrode plasma spraying equipment for hydrogen production by alkaline electrolyzed water

    CN121131117A

  • Low-overpotential high-activity catalyst coating for hydrogen production by electrolysis of water, preparation method and application of low-overpotential high-activity catalyst coating

    CN121250426A

  • Electrode catalyst, catalyst electrode and preparation method thereof

    CN121344644A

  • Plasma spraying device and method for nickel mesh electrode

    CN122147228A