Heat-proof wave-absorbing composite material as well as preparation method and application thereof
By adding absorbents and dispersants to the phenolic resin, a porous gelled structure is formed, which solves the problems of high density of thermal protection materials and easy failure of wave absorption functions in hypersonic aircraft, and achieves low density, heat insulation and full thickness absorption The composite material with wave function meets the lightweight and stealth needs of the aircraft.
Patent Information
- Application Number
- CN202410960617.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The existing thermal protection composite materials have high density and high thermal conductivity, which is difficult to meet the lightweight insulation needs of hypersonic aircraft. At the same time, the stealth wave absorption function is prone to failure in severe aerodynamic thermal environments, and the maintenance costs are high.
By adding absorbent, solvent and dispersant to the ablation-resistant phenolic resin, a suspension with good stability is formed, and it is poured into the fiber reinforced body by normal pressure or vacuum introduction method to form a porous gelled structure to achieve The uniform distribution of absorbents in phenolic aerogel composite materials reduces the density of the composite materials and enhances its absorbing properties.
The composite material with low density, heat insulation, ablation resistance and full thickness wave absorption functions is achieved, meeting the lightweight and stealth needs of hypersonic aircraft, and improving the ablation resistance and electromagnetic wave absorption performance of the material.
Smart Images

Figure CN118909395A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite materials, and in particular to a heat-proof and wave-absorbing composite material and a preparation method and application thereof. Background Art
[0002] Hypersonic aircraft need to design corresponding thermal protection materials to ensure the normal operation of the aircraft in the face of harsh aerodynamic thermal environments. At present, the low density of thermal protection materials is a major scientific and engineering technology issue that is constantly emphasized under the premise of meeting the heat protection needs. In addition to strict requirements on the density and thermal conductivity of thermal protection materials, modern high-speed aircraft also require thermal protection materials to have certain stealth and wave-absorbing properties. The stealth and heat protection of traditional aircraft are designed separately, and the corresponding wave-absorbing materials are attached to the surface of the heat protection layer. However, this method may cause the absorbing layer to be damaged or even the stealth and wave-absorbing function to fail when facing increasingly harsh aerodynamic thermal environments, and the maintenance cost is high. Therefore, how to achieve the integration of the heat protection layer and the wave-absorbing layer is an important topic in the research of high-speed aircraft, and it is also one of the development trends of high-performance thermal protection materials.
[0003] In order to achieve the integration of ablation resistance and wave absorption performance of thermal protection composite materials, the usual practice is to prepare functional layers such as ablation layer, thermal insulation layer, wave absorption layer, impedance matching layer, etc. separately, and then integrate them into a thermal protection and wave absorption composite material through a certain structural composite design. For example, the invention patent CN 112918025 A proposes an ablative thermal insulation and wave absorption integrated composite material and its preparation method, which obtains the corresponding composite material by sequentially stacking and curing a continuous fiber medium layer, a continuous fiber ablation layer, a continuous fiber thermal insulation layer, etc. The composite material obtained in this patent has good ablation resistance and wave absorption performance, but the overall density is still relatively high, reaching 1.4g / cm 3 , the thermal conductivity also reached 0.55 W / (m·K), which is difficult to meet the lightweight insulation requirements of thermal protection materials. Therefore, further reducing the density and thermal conductivity of thermal protection composite materials on the basis of meeting the ablation resistance performance is an important goal of high-performance thermal protection materials for hypersonic vehicles. Summary of the invention
[0004] In view of the above-mentioned deficiencies, the object of the present invention is to provide a heat-proof and wave-absorbing composite material and a preparation method and application thereof, so as to solve the problems of high density and high thermal conductivity of existing heat-protective composite materials.
[0005] To achieve the above object, the present invention is implemented through the following technical solutions: In a first aspect, the present invention provides a method for preparing a heat-resistant and wave-absorbing composite material, comprising the following steps: The ablation-resistant phenolic resin, the dispersant, the absorbent, the curing agent and the solvent are mixed to obtain an impregnation solution; soaking the fiber reinforcement in an impregnation liquid to obtain a prepreg; The prepreg is placed in a mold, and the impregnation liquid is passed into the mold until the fiber reinforcement is filled with the impregnation liquid; After the mold is sealed, the material is cured at 90-110° C. for 24-36 hours, and then demolded and dried to obtain a heat-resistant and wave-absorbing composite material.
[0006] Preferably, the ablation-resistant phenolic resin is linear phenolic resin and / or modified phenolic resin; the dispersant is at least one of polyvinyl pyrrolidone, silane coupling agent, titanate coupling agent, and Tween 80; the absorbent is one or more of carbon nanotubes, carbon black, graphene, silicon carbide, and carbonyl iron; the curing agent is hexamethylenetetramine; and the solvent is an alcohol solvent.
[0007] Preferably, the modified phenolic resin is one or more of boron phenolic resin, silicon phenolic resin, and multi-element hybrid phenolic resin; the particle size of the absorbent is less than 1 μm; and the alcohol solvent is at least one of ethanol, isopropanol, and n-propanol.
[0008] Preferably, the impregnation solution comprises, by weight, 20 to 60 parts of ablation-resistant phenolic resin, 1 to 10 parts of a dispersant, 5 to 20 parts of an absorbent, 3 to 10 parts of a curing agent, and 100 to 300 parts of a solvent.
[0009] Preferably, the dielectric constant of the fiber reinforcement is less than 5 and the volume density is 0.1-0.8 g / cm 3 .
[0010] Preferably, the fiber reinforcement is a flexible fiber felt or a fiber braid; the fiber material in the fiber reinforcement is at least one of quartz fiber, high silica fiber, alumina fiber, and zirconia fiber.
[0011] Preferably, the method of passing the impregnation liquid into the mold until the fiber reinforcement is filled with the impregnation liquid includes: introducing the impregnation liquid from one end of the mold under normal pressure or vacuum and leading it out from the other end of the mold. The fiber reinforcement is further filled with the impregnation liquid by normal pressure or vacuum impregnation and the bubbles are discharged.
[0012] Preferably, the drying method comprises: first drying at 50-60° C. for 24-48 hours, and then drying at 70-80° C. for 24-48 hours.
[0013] In a second aspect, the present invention provides a heat-resistant and wave-absorbing composite material, which is prepared by the preparation method described in the first aspect.
[0014] In a third aspect, the present invention provides an application of the above-mentioned heat-resistant and wave-absorbing composite material in a hypersonic aircraft.
[0015] The beneficial effects of the present invention are: The present invention integrates the ablation resistance, heat insulation and low density design of the thermal protection material with the wave absorbing functional design. On the basis of the fiber-reinforced phenolic aerogel composite material, an electromagnetic wave absorber is in-situ doped without affecting the pore structure and overall density of the composite material, thereby achieving low density, heat insulation, ablation resistance and excellent wave absorbing performance of the composite material.
[0016] The present invention improves the dispersibility of the absorbent in the resin solution by adding an active dispersant, and at the same time allows the absorbent to participate in the sol-gel reaction of phenolic formaldehyde, so that the absorbent is evenly distributed during the composite material molding process, thereby ensuring that the composite material has excellent thickness designability, can adapt to parts of different shapes and structures, and meet the heat protection and wave absorption performance of the thermal protection composite material under different aerodynamic thermal conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings of the embodiment are briefly introduced below.
[0018] Figure 1 This is a physical picture of the heat-resistant and wave-absorbing composite material prepared in Example 1 of the present invention; Figure 2 This is a graph showing the electromagnetic wave reflectivity of the heat-resistant and wave-absorbing composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] At present, the method to realize heat-proof and wave-absorbing functional materials is to introduce a wave-absorbing stealth coating on the surface of the thermal protection material. However, when the aircraft is flying at high speed, the coating is easily ablated by the high temperature environment caused by aerodynamic heat, resulting in the failure of stealth. It is impossible to achieve the full stealth function of hypersonic aircraft, and the thermal protection material must also have the characteristic of low density.
[0021] In order to improve the lightweight and stealth problems of hypersonic aircraft, the present invention provides an integrated composite material with heat-proof and wave-absorbing functions and a preparation method thereof. By adding an absorbent, a solvent and a curing agent to an ablation-resistant resin, and adding a dispersant to obtain a suspension with good stability, the suspension is infused into a fiber reinforcement by normal pressure or vacuum introduction. Finally, during the sealing and curing process, the presence of a large amount of solvent causes the phenolic resin to undergo polymerization-induced phase separation to form a porous gel structure, and a fiber-reinforced phenolic aerogel composite material is formed with the absorbent as the core. After normal pressure drying treatment, the solvent in the composite material is completely volatilized, and the absorbent is confined in the phenolic aerogel structure, so that the absorbent is evenly dispersed in the composite material. The obtained integrated composite material with heat-proof and wave-absorbing functions has the ablation resistance of phenolic, the heat insulation and light weight characteristics of the aerogel structure, and the electromagnetic wave absorption performance of the absorbent. Since the absorbent is also evenly distributed in the thickness direction of the composite material, the composite material also has good wave-absorbing performance during the ablation retreat process, realizing the full-thickness wave-absorbing function of the thermal protection material.
[0022] In order to further illustrate the present invention, the heat-resistant and wave-absorbing composite material provided by the present invention and its preparation method and application are described in detail below in combination with embodiments, but it should not be understood as limiting the protection scope of the present invention.
[0023] Example 1 1) According to parts by weight, 30 parts of phenolic resin are first dissolved in 100 parts of isopropanol solvent to form a dilute resin solution, and then 5 parts of polyvinyl pyrrolidone are added to the dilute resin solution, stirred to fully dissolve it, and then 15 parts of hydroxylated multi-walled carbon nanotubes and 5 parts of hexamethylenetetramine curing agent are added, and dispersed by an ultrasonic crusher for 30 minutes, and then mechanically stirred for 30 minutes to obtain a suspension precursor solution.
[0024] 2) The thickness is 10 mm and the volume density is 0.3 g / cm 3 The quartz fiber needle felt is completely immersed in the suspended precursor solution, so that the pores of the fiber reinforcement naturally absorb the precursor solution to a saturated state.
[0025] 3) Place the fiber reinforcement that has been fully absorbed with the precursor solution in a sealable metal mold and evacuate it. Pour the suspended precursor solution into the metal mold and continuously discharge it from the other end of the metal mold. Through vacuum impregnation, the fiber reinforcement is filled with the precursor solution and the bubbles are discharged.
[0026] 4) The metal mold is strictly sealed and placed in a constant temperature oven at 100°C for curing for 24 hours. The mold is then opened to take out the solvent-containing composite material, which is placed in a constant temperature oven for step-by-step normal pressure drying, drying at 60°C for 24 hours, and then drying at 80°C for 24 hours to obtain an integrated composite material with heat-resistant and wave-absorbing functions.
[0027] Figure 1 This is a physical picture of the heat-resistant and wave-absorbing composite material obtained in this example, in which various functional materials are evenly distributed. Figure 2 This is a graph showing the electromagnetic wave reflectivity of heat-resistant and wave-absorbing composite materials. It can be seen that in the frequency band of 4GHz~18GHz, the lowest reflectivity is nearly -20dB, and the average reflectivity is -8.9dB.
[0028] Example 2 1) According to parts by weight, 40 parts of boron phenolic resin are first dissolved in 150 parts of isopropanol solvent to form a resin dilute solution, and then 10 parts of silane coupling agent KH560 are added to the resin dilute solution, stirred to fully dissolve, and then 20 parts of nano carbonyl iron powder and 7 parts of hexamethylenetetramine curing agent are added, and dispersed by ultrasonic crusher for 30 minutes, and then mechanically stirred for 30 minutes to obtain a suspension precursor solution.
[0029] 2) The thickness is 5 mm and the volume density is 0.3 g / cm 3 The quartz fiber needle felt is completely immersed in the suspended precursor solution, so that the pores of the fiber reinforcement naturally absorb the precursor solution to a saturated state.
[0030] 3) Place the fiber reinforcement that has been fully absorbed with the precursor solution in a sealable metal mold and evacuate it. Pour the suspended precursor solution into the metal mold and continuously discharge it from the other end of the metal mold. Through vacuum impregnation, the fiber reinforcement is filled with the precursor solution and the bubbles are discharged.
[0031] 4) The metal mold is strictly sealed and placed in a constant temperature oven at 100°C for curing for 24 hours. The mold is then opened to take out the solvent-containing composite material, which is placed in a constant temperature oven for step-by-step normal pressure drying, drying at 60°C for 24 hours, and then drying at 80°C for 24 hours to obtain an integrated composite material with heat-resistant and wave-absorbing functions.
[0032] Example 3 1) According to parts by weight, 30 parts of phenolic resin are first dissolved in 100 parts of isopropanol solvent to form a dilute resin solution, and then 5 parts of Tween 80 are added to the dilute resin solution and stirred to fully dissolve it, and then 15 parts of nano-silicon carbide and 5 parts of hexamethylenetetramine curing agent are added, and dispersed by an ultrasonic crusher for 30 minutes, and then mechanically stirred for 30 minutes to obtain a suspension precursor solution.
[0033] 2) The thickness is 10 mm and the volume density is 0.3 g / cm 3 The quartz fiber needle felt is completely immersed in the suspended precursor solution, so that the pores of the fiber reinforcement naturally absorb the precursor solution to a saturated state.
[0034] 3) Place the fiber reinforcement that has been fully absorbed with the precursor solution in a sealable metal mold and evacuate it. Pour the suspended precursor solution into the metal mold and continuously discharge it from the other end of the metal mold. Through vacuum impregnation, the fiber reinforcement is filled with the precursor solution and the bubbles are discharged.
[0035] 4) The metal mold is strictly sealed and placed in a constant temperature oven at 100°C for curing for 24 hours. The mold is then opened to take out the solvent-containing composite material, which is placed in a constant temperature oven for step-by-step normal pressure drying, drying at 60°C for 24 hours, and then drying at 80°C for 24 hours to obtain an integrated composite material with heat-resistant and wave-absorbing functions.
[0036] Example 4 1) According to parts by weight, 60 parts of phenolic resin are first dissolved in 300 parts of isopropanol solvent to form a dilute resin solution, 10 parts of polyvinyl pyrrolidone are added to the dilute resin solution, stirred to fully dissolve, 20 parts of graphene oxide and 10 parts of hexamethylenetetramine curing agent are added, and the mixture is dispersed by an ultrasonic crusher for 30 minutes, and then mechanically stirred for 30 minutes to obtain a suspension precursor solution.
[0037] 2) The thickness is 5 mm and the volume density is 0.5 g / cm 3 The alumina needle felt fiber reinforcement is completely immersed in the suspended precursor solution, so that the pores of the fiber reinforcement naturally absorb the precursor solution to a saturated state.
[0038] 3) Place the fiber reinforcement that has been fully absorbed with the precursor solution in a sealable metal mold and evacuate it. Pour the suspended precursor solution into the metal mold and continuously discharge it from the other end of the metal mold. Through vacuum impregnation, the fiber reinforcement is filled with the precursor solution and the bubbles are discharged.
[0039] 4) The metal mold is strictly sealed and placed in a constant temperature oven at 100°C for curing for 24 hours. The mold is then opened to take out the solvent-containing composite material, which is placed in a constant temperature oven for step-by-step normal pressure drying, drying at 60°C for 24 hours, and then drying at 80°C for 24 hours to obtain an integrated composite material with heat-resistant and wave-absorbing functions.
[0040] The performance tests were performed on the composite materials prepared in Examples 1 to 4, and the results are shown in Table 1.
[0041] Table 1
[0042] As can be seen from Table 1, the composite material obtained by the present invention has low density, heat insulation, and ablation resistance, and at the same time exhibits excellent electromagnetic wave loss performance, realizing the integration of ablation, heat insulation, and wave absorption functions of thermal protection materials, thereby improving the lightweight and stealth problems of hypersonic aircraft.
[0043] In summary, the present invention adjusts the compatibility of the absorbent and the phenolic resin so that the absorbent has excellent dispersion stability in the phenolic resin, thereby achieving uniform distribution of the absorbent in the composite material. The composite material obtained by the present invention has ultra-lightweight, high porosity, ablation resistance, heat insulation and full-thickness wave absorbing functions, and can be applied to the molding of thermal protection materials with different thicknesses and complex structures, and can meet the needs of the aerospace field for stealth wave absorbing functional thermal protection materials.
[0044] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.
[0045] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a heat-resistant and wave-absorbing composite material, characterized in that: The following steps are involved: The ablation-resistant phenolic resin, the dispersant, the absorbent, the curing agent and the solvent are mixed to obtain an impregnation solution; soaking the fiber reinforcement in the impregnation liquid to obtain a prepreg; Placing the prepreg in a mold, and passing the impregnation liquid into the mold until the fiber reinforcement is filled with the impregnation liquid; After the mold is sealed, the material is cured at 90-110° C. for 24-36 hours, and then demoulded and dried to obtain the heat-resistant and wave-absorbing composite material.
2. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 1, characterized in that: The ablation-resistant phenolic resin is a linear phenolic resin and / or a modified phenolic resin; The dispersant is one or more of polyvinyl pyrrolidone, silane coupling agent, titanate coupling agent, and Tween 80; The absorbent is one or more of carbon nanotubes, carbon black, graphene, silicon carbide, and carbonyl iron; The curing agent is hexamethylenetetramine; The solvent is an alcohol solvent.
3. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 2, characterized in that: The modified phenolic resin is one or more of boron phenolic resin, silicon phenolic resin, and multi-element hybrid phenolic resin; the particle size of the absorbent is less than 1 μm; and the alcohol solvent is at least one of ethanol, isopropanol, and n-propanol.
4. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 1, characterized in that: In parts by weight, the impregnation liquid includes 20 to 60 parts of ablation-resistant phenolic resin, 1 to 10 parts of a dispersant, 5 to 20 parts of an absorbent, 3 to 10 parts of a curing agent, and 100 to 300 parts of a solvent.
5. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 1, characterized in that: The dielectric constant of the fiber reinforcement is less than 5, and the volume density is 0.1-0.8 g / cm 3 .
6. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 5, characterized in that: The fiber reinforcement is a flexible fiber felt or a fiber braid; the fiber material in the fiber reinforcement is at least one of quartz fiber, high silica fiber, alumina fiber and zirconia fiber.
7. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 1, characterized in that: The method of passing the impregnation liquid into the mold until the fiber reinforcement is filled with the impregnation liquid includes: introducing the impregnation liquid from one end of the mold under normal pressure or vacuum, and leading it out from the other end of the mold.
8. The method for preparing the heat-resistant and wave-absorbing composite material according to claim 1, characterized in that: The drying method comprises: first drying at 50-60° C. for 24-48 h, and then drying at 70-80° C. for 24-48 h.
9. A heat-resistant and wave-absorbing composite material, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. Use of the heat-resistant and wave-absorbing composite material according to claim 9 in a hypersonic aircraft.
Citation Information
Cited By
Heat prevention and insulation composite material as well as preparation method and application thereof
CN119613776A
Heat-insulating composite material, its preparation method and application
CN119613776B
Fiber-reinforced hybrid resin-based composite material and method of making and use thereof