High-heat-resistance binder for lithium ion battery diaphragm and preparation method of high-heat-resistance binder
By blending and preparing modified polyvinylidene fluoride-methacrylic-styrene terpolymer with PMMA and micron-scale polymer microspheres, the problem of the prone to short-circuit of lithium-ion battery separators at high temperatures is solved, and high The flame retardant, heat shrinkage resistance and mechanical strength of the heat-resistant adhesive ensure the safety performance of the battery.
Patent Information
- Application Number
- CN202411405718.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-08
AI Technical Summary
Existing lithium-ion battery separators are prone to battery short circuit after being heated, and lack flame retardancy, heat shrinkage resistance and mechanical strength, making it difficult to meet high performance needs.
High heat-resistant adhesive is prepared by blending modified polyvinylidene fluoride-methacrylic-styrene terpolymer with PMMA and micron-scale polymer microspheres. By regulating molecular weight and molar ratio, the adhesive is improved. Heat resistance, flame retardancy and mechanical strength.
The bonding ability between the diaphragm and the electrode sheet is significantly improved, the heat stability, flame retardancy and mechanical properties of the diaphragm are enhanced, the battery short circuit caused by high temperature is prevented, and the ionic conductivity is improved.
Smart Images

Figure SMS_5 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery technology, and in particular to a high heat-resistant adhesive for lithium ion battery separators and a preparation method thereof. Background Art
[0002] Lithium-ion battery is a high-performance rechargeable battery. It mainly relies on the movement of lithium ions between the positive and negative electrodes to work. The working principle of lithium-ion battery is that during the charging and discharging process, lithium ions are intercalated and deintercalated between the two electrodes. When charging, lithium ions are deintercalated from the positive electrode and embedded in the negative electrode through the electrolyte; when discharging, lithium ions are deintercalated from the negative electrode and embedded in the positive electrode through the electrolyte. This intercalation and deintercalation of lithium ions between the positive and negative electrodes realizes the charging and discharging process of the battery. The development of lithium-ion batteries can be traced back to the 1970s, but it was not until 1991 that Sony Corporation of Japan successfully developed the first commercial lithium-ion battery and applied it to electronic products such as laptops. Lithium-ion batteries began to gradually enter people's field of vision. Lithium-ion batteries have the remarkable characteristics of high energy density, long life, no memory effect, strong adaptability to high and low temperatures, green environmental protection, low self-discharge and long-term storage. Therefore, it is widely used in transportation, electronic products, energy storage systems, aviation and military fields.
[0003] Lithium-ion battery separator is one of the key components in lithium-ion batteries. Its main function is to separate the positive and negative electrodes of the battery to prevent the two electrodes from short-circuiting due to contact. At the same time, it maintains the necessary electrolyte during the electrochemical reaction to form a channel for ion movement. The performance of the separator directly affects the internal resistance, discharge capacity, cycle life and safety performance of the battery. The selection of separator materials is crucial to the overall performance of the battery. The main separator materials on the market currently include polyolefin separators, such as polyethylene, polypropylene and their composites. These materials are widely used due to their excellent mechanical properties, chemical stability and cost-effectiveness.
[0004] Conventional diaphragms can no longer meet the current social development needs. In order to overcome the shortcomings of polyolefin lithium battery diaphragms, more and more researchers have turned their attention to the process of diaphragm modification. A certain amount of binder needs to be added during diaphragm modification so that the diaphragm can better bond with the electrode. For example, the existing technologies with publication numbers CN115207566A, CN104140502A and CN115260403B all involve the use of binders in the preparation of diaphragms. However, due to the harsh environment in which the diaphragms are used, higher requirements are also placed on the performance of the binder.
[0005] For example, CN112072108A discloses “a conductive adhesive for lithium batteries and its preparation method” which is prepared by grafting 2-acrylamide-2-methylpropanesulfonic acid AMPS onto polyvinylidene fluoride PVDF through free radical polymerization and then blending with PMMA. The adhesive has good conductivity and certain thermal stability.
[0006] For example, CN115260403B discloses "a water-based binder, a modified diaphragm, a battery and a method for preparing a water-based binder". Self-made core-shell structured binder particles are coated on the surface of the diaphragm substrate to improve the strength of the battery and the air permeability of the diaphragm.
[0007] However, the above patents do not mention or solve the problem that the battery is prone to short circuit when the diaphragm shrinks due to heat.
[0008] Therefore, it is urgent to develop a high heat-resistant adhesive for lithium-ion battery separators that can improve the bonding ability between the separator and the electrode and has good flame retardancy, heat shrinkage resistance, ionic conductivity and mechanical strength. Summary of the invention
[0009] The main purpose of the present invention is to provide a high heat-resistant adhesive for lithium-ion battery separators and a preparation method thereof, wherein the adhesive can improve the bonding ability between the separator and the pole piece and has good flame retardancy, heat shrinkage resistance, conductivity and mechanical strength.
[0010] In order to achieve the above object, the technical solution adopted by the present invention is as follows: On one hand, the present invention provides a high heat-resistant adhesive for lithium-ion battery separators, comprising the following components in parts by weight: 48 to 52 parts of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, 12 to 16 parts of PMMA and 5 to 9 parts of micron-sized polymer microspheres.
[0011] The diaphragm is one of the key components in lithium-ion batteries. Its main function is to separate the positive and negative electrodes of the battery to prevent the two electrodes from short-circuiting due to contact. At the same time, it maintains the necessary electrolyte to form a channel for ion movement during the electrochemical reaction. The performance of the diaphragm directly affects the internal resistance, discharge capacity, cycle life and safety performance of the battery.
[0012] The diaphragm adhesive of the present application has high viscosity and can well bond the diaphragm and the pole piece. It also has certain heat resistance stability and heat shrinkage resistance, which can prevent the battery from short-circuiting due to temperature rise when used at high load. In addition, the adhesive can also give the diaphragm better flame retardancy, ionic conductivity and mechanical strength.
[0013] In some embodiments, the number average molecular weight of the PMMA is 550,000-750,000.
[0014] The present application regulates the number average molecular weight of PMMA to improve the viscosity of the adhesive, while preventing the molecular chain from decreasing in twisting ability and reducing the elasticity of the diaphragm.
[0015] In some embodiments, the number average molecular weight of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is 500,000-700,000.
[0016] The present application adjusts the number average molecular weight of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer to make it close to the molecular weight of PMMA, thereby improving the compatibility of the two and allowing the molecular chains of the two to be better interlaced. In addition, the applicant has found that the synergistic use of PMMA and the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer can further improve the heat resistance of the adhesive. The reason may be that PMMA and the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer chain segments are interlaced with each other, and the rigid side chains in the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer can inhibit the rotation of the PMMA main chain, thereby reducing the activity of the chain segments and further improving the heat resistance of the adhesive.
[0017] In some embodiments, the method for preparing the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer comprises the following steps: A1. Mix 1,4-cyclohexanedimethanol and potassium hydroxide solution, heat to 55-65°C, stir for 32-38 min, add epichlorohydrin dropwise, adjust the pH of the system to not less than 9, stir at constant temperature for 2-3 h, cool to 0-5°C after the reaction is completed, and adjust the pH of the system to neutral; A2, add 2-aminobenzenesulfonic acid to step A1, heat to 60-70°C, stir at constant temperature for 1-3h, cool to 0-5°C after the reaction, adjust the system pH to 1-2, and pass through a dialysis bag after the reaction to obtain the compound shown in formula I (I); A3, mixing the compound represented by formula I in step A2 with methacrylic acid, adding ethanol, adding concentrated sulfuric acid, heating to 50-60°C and stirring at constant temperature for 10-12 hours, cooling to room temperature after the reaction, concentrating under reduced pressure and drying to obtain monomer A; A4. Mix vinylidene fluoride, styrene and monomer A in step A3, add deionized water, add dispersant and initiator, raise the temperature to 80-90° C. and stir at constant temperature for 15-17 hours to obtain a modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer.
[0018] The modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer of the present application can improve the heat resistance and ionic conductivity of the binder, and at the same time can make the adhesion between the diaphragm and the electrode higher. The reason may be that, on the first aspect, the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer contains a large number of hydrogen bond donors and hydrogen bond acceptors, which cooperate with the hydrogen bonds in PMMA to better bond the diaphragm and the electrode together; on the second aspect, the side chain structure of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer contains a poly-2-aminobenzenesulfonic acid structure, which can cooperate with the pore structure formed by cross-linking the molecular chains of PMMA and the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, thereby greatly improving the ionic conductivity of the binder, and at the same time, the rigid structure therein can cooperate with PMMA to further improve the heat resistance of the binder; on the third aspect, the main chain structure of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer contains soft segment connections and hard segment connections, which ensures the flexibility of the diaphragm while improving the mechanical strength.
[0019] In some embodiments, in step A1, the molar ratio of 1,4-cyclohexanedimethanol to epichlorohydrin is 1:(0.8~1).
[0020] Preferably, in step A1, the molar ratio of 1,4-cyclohexanedimethanol to epichlorohydrin is 1:0.9.
[0021] The present application regulates the molar ratio of 1,4-cyclohexanedimethanol and epichlorohydrin, which can prevent the hydroxyl groups at both ends from reacting, resulting in an excessively high crosslinking density of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, thereby reducing the mechanical properties of the binder.
[0022] In some embodiments, the molar ratio of 2-aminobenzenesulfonic acid to 1,4-cyclohexanedimethanol is 1:(0.9-1).
[0023] Preferably, the molar ratio of 2-aminobenzenesulfonic acid to 1,4-cyclohexanedimethanol is 1:0.95.
[0024] In some embodiments, in step A3, the molar ratio of the compound represented by formula I to methacrylic acid is 1:(1-1.2).
[0025] Preferably, in step A3, the molar ratio of the compound represented by formula I to methacrylic acid is 1:1.1.
[0026] In some embodiments, in step A4, the mass ratio of vinylidene fluoride, styrene and monomer A is 1:(0.4~0.6):(0.7~0.9).
[0027] Preferably, in step A4, the mass ratio of vinylidene fluoride, styrene and monomer A is 1:0.5:0.8.
[0028] The present application can make the binder resistant to high temperatures and stable by regulating the mass ratio of vinylidene fluoride, styrene and monomer A while preventing the rigid side chains from causing a decrease in the toughness of the binder.
[0029] In some embodiments, the method for preparing the micron-sized polymer microspheres comprises the following steps: S1, mixing the mixed monomer A and the dispersant with an ethanol solution to prepare a monomer mixed solution; S2. In an inert gas atmosphere, the initiator and the monomer mixture in step S1 are mixed and emulsified, and the mixture is heated to 60-70° C. and stirred at a constant temperature for 1-2 hours to obtain a core layer emulsion; S3, mixing and dispersing the mixed monomer B and the emulsifier to obtain a shell emulsion; S4, dropwise adding the shell layer emulsion in step S3 to the core layer emulsion in step S2, adding an initiator, continuing to stir at a constant temperature for 23 to 26 hours, washing after the reaction is completed, and obtaining micron-sized polymer microspheres; The mixed monomer A includes styrene, norbornene-modified silica, methyl acrylate and hydroxyethyl methacrylate; The mixed monomer B includes 2-hydroxyethyl acrylate, carboxyethyl acrylate, ethylene glycol dimethacrylate and modified maleic anhydride.
[0030] In some embodiments, the method for preparing the norbornene-modified silica comprises the following steps: A1. Mix silica and thionyl chloride, add N,N-dimethylformamide, heat to 40-50°C and stir for 3-5h, cool to room temperature, quench, concentrate and dry under reduced pressure to obtain acyl chloride silica; A2. Under an inert gas atmosphere, 4-hydroxy-2-butanone and the acyl chloride silicon dioxide in step A1 are mixed, added with acetone for dispersion, an acid binding agent is added, the temperature is raised to 40-60° C. and stirred at a constant temperature for 12-14 hours. After the reaction is completed, the mixture is filtered, concentrated and dried under reduced pressure to obtain keto-modified silicon dioxide; A3. Mix the keto-modified silica in step A2 with 5-norbornene-2-methylamine, add methanol, add an acid binding agent, heat to 60-70° C. and stir at a constant temperature for 6-8 hours. After the reaction is completed, filter to obtain norbornene-modified silica.
[0031] In some embodiments, the preparation method of the modified maleic anhydride comprises the following steps: mixing maleic anhydride with 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-ethanol 10-oxide and 1-naphthylethanol, adding chloroform to disperse, then heating to 55-60°C and stirring at a constant temperature for 8-10 hours. After the reaction is completed, column chromatography is performed to obtain modified maleic anhydride, whose structural formula is shown in Formula I (I).
[0032] On the other hand, the present invention provides a method for preparing a high heat-resistant adhesive for lithium-ion battery separators, comprising the following steps: mixing modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer and PMMA at 20-30° C. and stirring for 20-30 minutes, then adding micron-sized polymer microspheres and stirring at 500-700 r / min for 30-40 minutes to obtain the high heat-resistant adhesive.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The present invention adopts modified polyvinylidene fluoride-methyl methacrylate-styrene terpolymer, PMMA and micron-sized polymer microspheres to prepare a high heat-resistant adhesive for lithium-ion battery separators. The synergistic effect between the components of the adhesive can improve the bonding ability between the separator and the electrode, and has good flame retardancy, heat shrinkage resistance, ionic conductivity and mechanical strength.
[0035] (2) The modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer of the present invention, on the one hand, contains a large number of hydrogen bond donors and hydrogen bond acceptors in its structure, which cooperate with the hydrogen bonds in PMMA to better bond the diaphragm and the electrode together; on the other hand, the side chain structure of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer contains a poly 2-aminobenzenesulfonic acid structure, which can cooperate with the pore structure formed by cross-linking the molecular chains of PMMA and the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, thereby greatly improving the ionic conductivity of the binder. At the same time, the rigid structure therein can cooperate with PMMA to further improve the temperature resistance of the binder; on the third hand, the main chain structure of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer contains soft segment links and hard segment links, which ensure the flexibility of the diaphragm while improving the mechanical strength.
[0036] (3) The micron-sized polymer microspheres of the present invention can improve the heat resistance and mechanical properties of the adhesive and can also resist high temperature shrinkage. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The median particle size of the micron-sized polymer microspheres was measured using a Mastersizer 2000 laser particle size analyzer; the number average molecular weight was measured using a BOCL104 gel permeation chromatograph (GPC) produced by Shimadzu Corporation.
[0039] In the following preparation examples, embodiments and comparative examples, polyvinyl pyrrolidone was purchased from Jinan Yuyi Chemical Co., Ltd.; the CAS number of PMMA is 9011-14-7.
[0040] Preparation Example 1 A method for preparing norbornene-modified silicon dioxide comprises the following steps: A1. Mix 10 g of silica with 100 mL of thionyl chloride, add 0.5 mL of N,N-dimethylformamide, heat to 45 °C and stir for 4 h, cool to 27 °C, quench, and concentrate and dry under reduced pressure to obtain acyl chloride silica; A2. Under N2 atmosphere, 5 g (56 mmol) of 4-hydroxy-2-butanone and 11 g of the acyl chloride silica prepared in step A1 were mixed and dispersed in 200 mL of acetone, and 72 mmol of triethylamine was added. The mixture was heated to 50° C. and stirred at constant temperature for 13 h. After the reaction was completed, the mixture was filtered, concentrated under reduced pressure, and dried to obtain keto-modified silica. A3. Mix the keto-modified silica in step A2 with 2.7 g (22 mmol) of 5-norbornene-2-methylamine, add 50 mL of methanol, add 29 mmol of triethylamine, raise the temperature to 65° C. and stir at this temperature for 7 h. After the reaction is completed, filter to obtain norbornene-modified silica.
[0041] Preparation Example 2 The preparation method of modified maleic anhydride comprises the following steps: 80 mmol of maleic anhydride is mixed with 96 mmol of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-ethanol 10-oxide and 76 mmol of 1-naphthylethanol, 100 mL of chloroform is added for dispersion, and then the mixture is heated to 57° C. and stirred at a constant temperature for 9 hours. After the reaction is completed, the modified maleic anhydride is obtained by column chromatography, and the structural formula thereof is shown in Formula I. (I).
[0042] Preparation Example 3 The method for preparing micron-sized polymer microspheres comprises the following steps: S1, mixing 10 g of mixed monomer A and 1.5 g of polyvinyl pyrrolidone with 150 mL of ethanol solution to prepare a monomer mixture; S2. Under N2 atmosphere, 0.15 g of azobisisobutyronitrile and the monomer mixture in step S1 were mixed and emulsified, and the mixture was heated to 65° C. and stirred at the constant temperature for 1.5 h to obtain a core layer emulsion; S3, 30g of mixed monomer B and 0.6g of sodium dodecyl sulfate were mixed and dispersed to obtain a shell emulsion; S4, dropwise adding the shell layer emulsion in step S3 to the core layer emulsion in step S2, and adding 0.6 g of sodium persulfate, and continuing stirring at 65° C. for 24 h. After the reaction is completed, washing is performed to obtain micron-sized polymer microspheres; Wherein, the mixed monomer A comprises styrene, norbornene-modified silica, methyl acrylate and hydroxyethyl methacrylate in a mass ratio of 1:0.3:0.8:0.09; the mixed monomer B comprises 2-hydroxyethyl acrylate, carboxyethyl acrylate, ethylene glycol dimethacrylate and modified maleic anhydride in a mass ratio of 1:0.4:0.15:0.4; the norbornene-modified silica is prepared by Preparation Example 1, and the modified maleic anhydride is prepared by Preparation Example 2. The average particle size is 2.5629 μm.
[0043] Preparation Example 4 The preparation method of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer comprises the following steps: A1. Mix 0.5 mol 1,4-cyclohexanedimethanol and 100 mL 16 wt% potassium hydroxide solution, heat to 60 °C and stir for 36 min, add 0.45 mol epichlorohydrin dropwise, add 16 wt% potassium hydroxide solution to adjust the pH of the system to 9, stir at constant temperature for 2.5 h, cool to 2 °C after the reaction is completed, and adjust the pH of the system to 7 with 2 mol / L hydrochloric acid solution; A2, add 0.53 mol 2-aminobenzenesulfonic acid to step A1, heat to 65°C, stir at constant temperature for 2h, cool to 2°C after the reaction, adjust the system pH to 1 with 1 mol / L hydrochloric acid solution, and pass through a dialysis bag after the reaction to obtain the compound shown in formula I (I); A3, 0.5 mol of the compound represented by formula I in step A2 was mixed with 0.55 mol of methacrylic acid, 1 L of ethanol was added, 28 g of 98 wt% concentrated sulfuric acid was added, the temperature was raised to 55° C. and stirred for 11 h. After the reaction was completed, the temperature was lowered to 27° C., and the temperature was concentrated and dried under reduced pressure to obtain monomer A; A4, 10g of vinylidene fluoride, 5g of styrene and 8g of monomer A in step A3 were mixed and added into 100mL of deionized water, 0.01g of methyl cellulose ether and 0.04g of diethyl peroxydicarbonate were added thereto, the temperature was raised to 850°C and stirred at constant temperature for 16h to obtain a modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer with a number average molecular weight of 652800.
[0044] Preparation Example 5 The preparation method of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is the same as that of Preparation Example 4, except that the amount of epichlorohydrin is 1 mol and the number average molecular weight is 589600.
[0045] Preparation Example 6 The preparation method of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is the same as that of Preparation Example 4, except that the amount of monomer A is 13 g and the number average molecular weight is 698,400.
[0046] Preparation Example 7 The preparation method of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is the same as that of Preparation Example 4, except that equimolar aniline is used instead of 2-aminobenzenesulfonic acid. The number average molecular weight is 652700.
[0047] Preparation Example 8 The preparation method of polyvinylidene fluoride-methacrylic acid-styrene terpolymer is the same as that of Preparation Example 4, except that an equal amount of methacrylic acid is used to replace monomer A. The number average molecular weight is 526100.
[0048] Preparation Example 9 The preparation method of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is the same as that of Preparation Example 4, except that the amount of styrene is 9 g and the number average molecular weight is 615800.
[0049] Example 1 A high heat-resistant adhesive for lithium-ion battery separators, comprising the following components by weight: 50 parts of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, 14 parts of PMMA and 7 parts of micron-sized polymer microspheres; Wherein, the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 4, the micron-sized polymer microspheres are prepared by Preparation Example 3, and the number average molecular weight of PMMA is 650000; The preparation method of a high heat-resistant adhesive for lithium-ion battery separators comprises the following steps: mixing and stirring a modified polyvinylidene fluoride-methyl acrylate-styrene terpolymer and PMMA at 25°C for 25 minutes, then adding micron-sized polymer microspheres and stirring at 600 r / min for 35 minutes to obtain a high heat-resistant adhesive.
[0050] Example 2 A high heat-resistant binder for lithium-ion battery separators, comprising the following components by weight: 48 parts of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, 12 parts of PMMA and 5 parts of micron-sized polymer microspheres; Among them, the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 4, the micron-sized polymer microspheres are prepared by Preparation Example 3, and the number average molecular weight of PMMA is 550000; The preparation method of a high heat-resistant adhesive for lithium-ion battery separators comprises the following steps: mixing and stirring a modified polyvinylidene fluoride-methyl methacrylate-styrene terpolymer and PMMA at 20°C for 30 minutes, then adding micron-sized polymer microspheres and stirring at 500 r / min for 40 minutes to obtain a high heat-resistant adhesive.
[0051] Example 3 A high heat-resistant binder for lithium-ion battery separators, comprising the following components by weight: 52 parts of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, 16 parts of PMMA and 9 parts of micron-sized polymer microspheres; Wherein, the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 4, the micron-sized polymer microspheres are prepared by Preparation Example 3, and the number average molecular weight of PMMA is 750000; The preparation method of a high heat-resistant adhesive for lithium-ion battery separators comprises the following steps: mixing and stirring a modified polyvinylidene fluoride-methyl acrylate-styrene terpolymer and PMMA at 30°C for 20 minutes, then adding micron-sized polymer microspheres and stirring at 700 r / min for 30 minutes to obtain a high heat-resistant adhesive.
[0052] Example 4 A high heat-resistant adhesive for lithium-ion battery separator and a preparation method thereof. The specific implementation method is the same as Example 1, except that the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 5.
[0053] Example 5 A high heat-resistant adhesive for lithium-ion battery separator and a preparation method thereof. The specific implementation method is the same as Example 1, except that the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 6.
[0054] Example 6 A high heat-resistant adhesive for lithium-ion battery separator and a preparation method thereof. The specific implementation method is the same as Example 1, except that the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 7.
[0055] Example 7 A high heat-resistant binder for lithium-ion battery separator and a preparation method thereof. The specific implementation method is the same as Example 1, except that the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 9.
[0056] Example 8 A high heat-resistant adhesive for lithium-ion battery separator and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the number average molecular weight of PMMA is 300,000.
[0057] Comparative Example 1 A high heat-resistant adhesive for lithium-ion battery separator and a preparation method thereof. The specific implementation method is the same as Example 1, except that an equal mass portion of polyvinylidene fluoride-methacrylic acid-styrene terpolymer is used instead of a modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, and the polyvinylidene fluoride-methacrylic acid-styrene terpolymer is prepared by Preparation Example 8.
[0058] Performance Test: (1) Peel strength: The positive electrode sheet is composed of 200 parts of lithium manganese oxide + 150 parts of lithium iron phosphate + 10 parts of conductive carbon black + 16 parts of PVDF. The positive electrode sheet and the polypropylene separator coated with 2μm binder are hot pressed at 85℃ and 3MPa for 60s. After hot pressing, the test samples are cut into 25×200mm size and the peel strength is tested using KT-PSA-1056 peel force tester; (2) Elongation test: Cut the separator in method (1) into dumbbell-shaped specimens with a width of 20 mm, a narrow part width of 10 mm, a narrow parallel part length of 80 mm, and a total length of 150 mm. Use a universal mechanical testing machine to stretch at a speed of 1 mm / min and perform an elongation test with reference to GB / T36363-2018 "Polyolefin separators for lithium-ion batteries"; (3) Transverse heat shrinkage resistance: Tested according to the method of Q / 320405BCP001-2021 "Low heat shrinkage ceramic coated lithium ion battery separator", test conditions: 120°C for 1h; (4) Heat resistance and stability: The separator in method (1) of the present application is assembled into a battery with reference to the method in patent number CN117937049A, and the battery obtained is tested with reference to the "battery thermal stability test" therein; (5) Ionic conductivity: The membrane sample in method (1) was made into a 2016 button battery, the electrolyte was EC:DEC=1:1, and the concentration of LiPF6 was 1 mol / L. The ionic conductivity was calculated by the following formula through the AC impedance test in the electrochemical workstation: σ = d / (R b S); Where d is the sample thickness, R b is the body resistance, and S is the effective diaphragm area.
[0059] The high heat-resistant adhesives of the embodiments and comparative examples were tested according to the above test method. The results are shown in Table 1.
[0060] Table 1
[0061] According to the above results, it is found that the high heat-resistant adhesives of Examples 1 to 3 have strong bonding force, excellent mechanical properties, good resistance to heat shrinkage, and good heat stability and ionic conductivity; in Example 4, due to the change in the molar ratio of 1,4-cyclohexanedimethanol and epichlorohydrin, both hydroxyl groups in 1,4-cyclohexanedimethanol react, resulting in excessive crosslinking density of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, thereby reducing the tensile properties of the diaphragm; in Example 5, due to the change in the mass ratio of vinylidene fluoride, styrene and monomer A, the increase in rigid side chains leads to a decrease in the elongation of the adhesive, but the increase in rigid side chain groups enhances the synergistic effect on PMMA, reduces the activity of the chain segments, and thus improves the adhesive. The high temperature resistance of the binder is improved, and the increase of sulfonic acid groups improves the ionic conductivity of the binder; in Example 6, aniline is used in equal moles instead of 2-aminobenzenesulfonic acid, and the ionic conductivity of the binder decreases due to the lack of sulfonic acid groups; in Example 7, the elongation of the binder decreases, but the heat resistance is increased due to the change in the mass ratio of vinylidene fluoride, styrene and monomer A; in Comparative Example 1, the ionic conductivity and high temperature stability of the binder are significantly reduced due to the use of equal mass parts of polyvinylidene fluoride-methacrylic acid-styrene terpolymer instead of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer. In addition, due to the shortening of the side chain, the synergistic effect on PMMA is weakened, resulting in a decrease in heat resistance.
[0062] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A high heat-resistant binder for lithium-ion battery separator, characterized in that: The invention comprises the following components in parts by weight: 48 to 52 parts of modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer, 12 to 16 parts of PMMA and 5 to 9 parts of micron-sized polymer microspheres.
2. The high heat-resistant binder for lithium-ion battery separator according to claim 1, characterized in that: The number average molecular weight of the PMMA is 550,000-750,000.
3. The high heat-resistant binder for lithium-ion battery separator according to claim 1, characterized in that: The number average molecular weight of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer is 500,000-700,000.
4. The high heat-resistant binder for lithium-ion battery separator according to claim 1, characterized in that: The preparation method of the modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer comprises the following steps: A1. Mix 1,4-cyclohexanedimethanol and potassium hydroxide solution, heat to 55-65°C, stir for 32-38 min, add epichlorohydrin dropwise, adjust the pH of the system to not less than 9, stir at constant temperature for 2-3 h, cool to 0-5°C after the reaction is completed, and adjust the pH of the system to neutral; A2, add 2-aminobenzenesulfonic acid to step A1, heat to 60-70°C, stir at constant temperature for 1-3h, cool to 0-5°C after the reaction, adjust the system pH to 1-2, and pass through a dialysis bag after the reaction to obtain the compound shown in formula I (Ⅰ); A3, mixing the compound represented by formula I in step A2 with methacrylic acid, adding ethanol, adding concentrated sulfuric acid, heating to 50-60°C and stirring at constant temperature for 10-12 hours, cooling to room temperature after the reaction, concentrating under reduced pressure and drying to obtain monomer A; A4. Mix vinylidene fluoride, styrene and monomer A in step A3, add deionized water, add dispersant and initiator, raise the temperature to 80-90° C. and stir at constant temperature for 15-17 hours to obtain a modified polyvinylidene fluoride-methacrylic acid-styrene terpolymer.
5. The high heat-resistant binder for lithium-ion battery separator according to claim 4, characterized in that: In step A1, the molar ratio of 1,4-cyclohexanedimethanol to epichlorohydrin is 1:(0.8~1).
6. The high heat-resistant binder for lithium-ion battery separator according to claim 4, characterized in that: The molar ratio of the 2-aminobenzenesulfonic acid to 1,4-cyclohexanedimethanol is 1:(0.9-1).
7. The high heat-resistant binder for lithium-ion battery separator according to claim 4, characterized in that: In step A3, the molar ratio of the compound represented by formula I to methacrylic acid is 1:(1-1.2).
8. The high heat-resistant binder for lithium-ion battery separator according to claim 4, characterized in that: In step A4, the mass ratio of vinylidene fluoride, styrene and monomer A is 1:(0.4-0.6):(0.7-0.9).
9. The high heat-resistant binder for lithium-ion battery separator according to claim 1, characterized in that: The method for preparing the micron-sized polymer microspheres comprises the following steps: S1, mixing the mixed monomer A and the dispersant with an ethanol solution to prepare a monomer mixed solution; S2. In an inert gas atmosphere, the initiator and the monomer mixture in step S1 are mixed and emulsified, and the mixture is heated to 60-70° C. and stirred at a constant temperature for 1-2 hours to obtain a core layer emulsion; S3, mixing and dispersing the mixed monomer B and the emulsifier to obtain a shell emulsion; S4, dropwise adding the shell layer emulsion in step S3 to the core layer emulsion in step S2, adding an initiator, continuing to stir at a constant temperature for 23 to 26 hours, washing after the reaction is completed, and obtaining micron-sized polymer microspheres; The mixed monomer A includes styrene, norbornene-modified silica, methyl acrylate and hydroxyethyl methacrylate; The mixed monomer B includes 2-hydroxyethyl acrylate, carboxyethyl acrylate, ethylene glycol dimethacrylate and modified maleic anhydride.
10. A method for preparing a high heat-resistant binder for lithium-ion battery separator according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing modified polyvinylidene fluoride-methyl acrylate-styrene terpolymer and PMMA at 20-30°C for 20-30 minutes, then adding micron-sized polymer microspheres and stirring at 500-700 r / min for 30-40 minutes to obtain a high heat-resistant adhesive.
Citation Information
Patent Citations
Water-based slurry for high-cohesiveness separator and lithium-ion battery separator manufactured by using water-based slurry
CN110760279A
Modified binder as well as preparation method and application thereof
CN116904147A
Electrode binder comprising blend of polybutadiene-based polymer and polynorbornene-based polymer, electrode comprising same and use thereof in electrochemistry
CN117413387A
High-temperature-resistant flame-retardant ceramic coating diaphragm water-based binder as well as preparation method and application thereof
CN117987046A
Binder, preparation method, positive electrode plate, secondary battery, and electric device
WO2024066504A1
Cited By
PMMA (polymethyl methacrylate) glue with high ionic conductivity and preparation method thereof
CN119775930A
Binder for coating lithium battery current collector and preparation method thereof
CN119823656A
Uniform high-adhesion PMMA (polymethyl methacrylate) material for lithium battery diaphragm and preparation method of uniform high-adhesion PMMA material
CN119931559A