Smelting method of boron-containing steel for neutron shielding material
Through the dual-connection process of vacuum smelting and electroslag remelting, the problems of precision composition and structural uniformity in the smelting of boron-containing steel for neutron shielding materials are solved, and a low-cost and efficient smelting process is achieved, and the processing performance of the material is improved. Suitable for industrial production.
Patent Information
- Application Number
- CN202411226601.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The existing smelting method of boron-containing steel for neutron shielding materials has the problem of precise component control and difficult to achieve tissue uniformity, and the preparation process is complex and costly.
Using the dual process of vacuum smelting and electroslag remelting, the B content and the argon gas charging pressure are accurately controlled through the reasonable refining time during vacuum smelting and the six-melt slag system and low-melt smelting during electroslag remelting, and the B content and Elemental uniformity.
It realizes precise control of elements and tissue uniformity in liquid steel, reduces the content of harmful gases and elements, simplifies the smelting process, improves the hot and cold processing performance of the materials, and is suitable for industrial production.
Smart Images

Figure CN118910491A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of special materials, in particular to a method for smelting boron-containing steel for neutron shielding materials. Background Art
[0002] Boron steel for neutron shielding is a special boron steel, which is mostly used as control rods and thermal neutron shielding materials for nuclear reactors and nuclear waste storage racks. It is based on stainless steel and uses iron, which has good shielding performance for gamma radiation, as the matrix. Combined with the nuclear properties of B's superior shielding of thermal neutrons and suppression of captured gamma rays, boron steel has both neutron and gamma ray comprehensive shielding performance. At present, boron-containing stainless steel has become one of the indispensable protective materials in radiation protection design devices.
[0003] Generally speaking, boron-containing steel for neutron shielding materials can be prepared by two methods: smelting and hot isostatic pressing. The hot isostatic pressing method uses natural ferroboron powder and 304 stainless steel powder as raw materials, obtains nearly fully dense block materials through hot isostatic pressing, and then obtains them through forging and hot rolling. The preparation process is complicated and the cost is relatively high. The smelting method is to prepare it through smelting methods such as electric furnaces, non-vacuum induction furnaces, and vacuum induction furnaces. However, the precise control of boron content and the uniformity of the organization are the limiting conditions for the smelting of boron-containing steel. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for smelting boron-containing steel for neutron shielding material with precise composition and uniform structure.
[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: it includes vacuum smelting and electroslag remelting processes;
[0006] The vacuum smelting process: The vacuum smelting process: After refining, 10000~30000Pa argon gas is filled into the furnace, and alloying is carried out after the filling is completed. The alloying time is ≥0.5× M is the mass of molten steel smelted in the vacuum furnace, kg;
[0007] The electroslag remelting process: the slag system used is pre-melted slag and Al powder, the pre-melted slag contains B2O3; the content [B2O3]% of B2O3 in the pre-melted slag is determined according to the B content in the vacuum ingot, Wherein, a is the percentage of B in the vacuum ingot; the amount of Al powder added is 0.2% to 0.4% of the mass of the pre-melted slag.
[0008] Furthermore, in the electroslag remelting process, the pre-melted slag has the following components: CaF2 40% to 47%, CaO 20% to 25%, MgO 3% to 5%, Al2O3 20% to 25%, SiO2 4% to 7% and B2O3.
[0009] Furthermore, in the vacuum smelting process, the tapping temperature of the molten steel is 40 to 60° C. above the liquidus.
[0010] Furthermore, in the electroslag remelting process, the melting rate v is controlled to be (0.013-0.015)×D during the constant melting rate melting process. 结 , where v is the melting rate, kg / min, and D is the diameter of the electroslag furnace crystallizer, mm.
[0011] The beneficial effects of the above technical solution are as follows: the present invention innovatively adopts vacuum induction + electroslag remelting dual smelting process for preparation. In the vacuum smelting process, by designing a reasonable refining time and making full use of the vacuum carbon deoxidation capacity, the O, N, H gas content in the molten steel and harmful elements in the steel are reduced to the maximum extent, creating favorable conditions for the subsequent alloying process; and in the alloying process, by adjusting the furnace pressure and alloying time, the B content is precisely controlled. In the electroslag remelting process, a six-element slag system is designed, and by adding a certain proportion of B2O3, SiO2 and Al powder to the fixed slag system, the oxidation and burning of B and Si elements in the electroslag process are effectively suppressed, and the content of each element is precisely controlled; further, the electroslag process is controlled by low melting speed, which fully guarantees the uniformity of the electroslag solidification structure and composition, and guarantees the hot and cold processing performance of the material in the subsequent hot processing process.
[0012] The present invention effectively controls the quality of the ingot from the beginning of vacuum smelting, effectively ensures the uniformity of the solidification structure and composition of the electroslag product, improves the cold and hot processing performance of the material, and has simple smelting process operation, which is of great significance to the industrialized and stable production of such products. DETAILED DESCRIPTION
[0013] The present invention is further described in detail below in conjunction with specific implementation modes.
[0014] The present invention discloses a smelting method of boron-containing steel for neutron shielding material, wherein the chemical composition of the boron-containing steel is as follows: Si 0.2% to 2%, Mn 0.5% to 3%, Ni 11% to 15%, Cr 5% to 20%, B 0.5% to 3%, P≤0.02%, S≤0.02%, and the rest is Fe and unavoidable impurity elements. The smelting method adopts vacuum smelting and electroslag remelting process, and the process steps are as follows:
[0015] (1) Vacuum smelting process: including batching, furnace loading, melting, refining, alloying and pouring;
[0016] (1.1) Ingredients: The vacuum smelting materials are calculated according to the composition requirements of boron-containing steel. Industrial pure materials are used as the main raw materials. Industrial pure iron, electrolytic nickel plate, metallic chromium, carbon powder, industrial silicon, electrolytic manganese and ferroboron are selected. All elements in the metal materials are considered and the ingredients are accurately calculated.
[0017] (1.2) Furnace loading: Place nickel plate and metal chromium at the bottom of the crucible of the vacuum furnace, and pure iron in the middle; load carbon powder, industrial silicon, electrolytic manganese and ferroboron into the secondary silo; dry the chute and ingot mold and place them in the corresponding positions.
[0018] (1.3) Melting: Evacuate the chamber to a vacuum degree of ≤5Pa, and apply electric heating until the steel in the crucible is completely melted.
[0019] (1.4) Refining process: After all the metal materials in the crucible are melted, refining begins and carbon powder and industrial silicon are added to the molten steel. The refining time is not less than M is the mass of molten steel smelted in the vacuum furnace, unit: kg.
[0020] (1.5) Alloying refining process: After refining, 10000~30000Pa argon gas is filled into the furnace. After the filling is completed, electrolytic manganese and ferroboron are added for alloying. The alloying time is not less than M is the mass of molten steel smelted in the vacuum furnace, unit: kg.
[0021] (1.6) Casting process: After the composition test is qualified, the tapping temperature of the molten steel is adjusted to 40-60℃ above the liquidus line, and the casting is carried out under electricity. The ingot can be demoulded after it is completely solidified.
[0022] (2) Electroslag remelting process: pre-smelting preparation, arcing and slag removal, and constant melting rate smelting are adopted, and argon gas protection is used throughout the process;
[0023] (2.1) Preparation before smelting: Cut off the cap of the vacuum smelting ingot to ensure that there is no shrinkage cavity at the end and that there is no oxide layer on the surface of the ingot. If necessary, grind the surface and weld it to the auxiliary electrode after pretreatment;
[0024] A slag system is prepared, wherein the slag system is pre-melted slag and Al powder added separately; the mass percentage of the pre-melted slag components is: CaF2 40%-47%, CaO 20%-25%, MgO 3%-5%, Al2O3 20%-25%, SiO2 4%-7% and B2O3; the B2O3 content is determined according to the B content in the vacuum ingot, Wherein, a is the mass percentage of B in the vacuum ingot, [B2O3]% is the mass percentage of B2O3 in the pre-melted slag. The amount of Al powder added is 0.2% to 0.4% of the mass of the pre-melted slag. The pre-melted slag is stirred and mixed, and then placed in a heating furnace for baking for use, and Al powder is added before use.
[0025] (2.2) Arcing and slag-forming process: Place an ingot starter plate of the same material on the electroslag bottom water tank, place arc starting chips of the same material in the center of the ingot starter plate, install the crystallizer, protective fume hood, and consumable electrode, turn on the power to start the arc, and slowly add the slag material of the above slag system after the arc light stabilizes.
[0026] (2.3) Constant melting rate smelting process: After slag melting, control the melting rate v = (0.013 ~ 0.015) × D 结 , where v is the melting rate, in kg / min; D 结 It is the diameter of the electroslag furnace crystallizer, in mm. When the consumable electrode remains a certain weight after smelting, the shrinkage is fed. After the shrinkage is finished, the smelting power is turned off. After the electroslag ingot is completely solidified, it can be demoulded to obtain the boron-containing steel electroslag ingot. During the entire smelting period, argon gas is continuously introduced as a protective gas, and the atmosphere pressure is guaranteed to be 500Pa or more above the atmospheric pressure, ensuring that the oxygen in the atmosphere is ≤10ppm during the entire smelting process.
[0027] Embodiment 1:
[0028] (1) A 500Kg vacuum induction furnace and a 1t protective atmosphere electroslag furnace were used to carry out 3 furnaces of smelting, namely 1#, 2# and 3#, and the target values of smelting composition are shown in Table 1-1;
[0029] Table 1-1: Chemical composition target of Example 1 (wt%)
[0030]
[0031]
[0032] In Table 1, the balance is Fe and inevitable impurity elements.
[0033] (2) The vacuum smelting process: the casting ingot mold is Φ220×1700mm. The mass of the molten steel smelted in the vacuum furnace is 500kg; the refining time is not less than Alloying time is not less than
[0034]
[0035] The electroslag remelting process: the crystallizer is Φ300×1500mm. The total mass of the pre-melted slag is 25kg, and the B2O3 content in the pre-melted slag is The amount of Al powder added is 25×(0.2~0.4)%=0.05kg~0.1kg. The melting rate is controlled to be (0.013~0.015)×D 结 =(0.013~0.015)×300=3.9kg / min~4.5kg / min.
[0036] The smelting process parameters of the 1# to 3# heats of this embodiment are shown in Table 1-2, and the slag components of the 1# to 3# heats are shown in Table 1-3;
[0037] Table 1-2: Smelting process parameters of Example 1
[0038]
[0039] In Table 2, TL is the liquidus temperature.
[0040] Table 1-3: Slag composition of Example 1
[0041]
[0042] (3) After demoulding, the electroslag ingot was sliced at a distance of 200 mm from the bottom, and two samples were taken from the center of the cross section, at R / 2, and at the edge for chemical composition testing. The chemical composition test results are shown in Table 1-4;
[0043] Table 1-4: Chemical composition test results of 1# to 3# electroslag ingots in Example 1 (wt%)
[0044]
[0045]
[0046] Through organizational observation and chemical composition testing, the electroslag ingots obtained from 1# to 3# heats have qualified compositions, and the solidified structure and composition are uniform.
[0047] Embodiment 2:
[0048] (1) A 1.5t vacuum induction furnace and a 1.5t protective atmosphere electroslag furnace were used to carry out 3 furnaces of smelting, namely 1#, 2# and 3#. The target values of smelting composition are shown in Table 2-1;
[0049] Table 2-1: Chemical composition target of Example 2 (wt%)
[0050] To Mn P S Cr In B 2 0.5 ≤0.02 ≤0.02 5 15 3
[0051] In Table 1, the balance is Fe and inevitable impurity elements.
[0052] (2) The vacuum smelting process: the casting ingot mold is selected as Φ380×1800mm ingot. The mass of the molten steel smelted in the vacuum furnace is 1500kg; the refining time is not less than Alloying time is not less than
[0053] The electroslag remelting process: the crystallizer is Φ500×1000mm. The total mass of the pre-melted slag is 85kg, and the B2O3 content in the pre-melted slag is The amount of Al powder added is 85×(0.2~0.4)%=0.17kg~0.34kg. The melting rate is controlled to be (0.013~0.015)×D 结 =(0.013~0.015)×500=6.5kg / min~7.5kg / min.
[0054] The smelting process parameters of the 1# to 3# heats of this embodiment are shown in Table 2-2, and the slag components of the 1# to 3# heats are shown in Table 2-3;
[0055] Table 2-2: Smelting process parameters of Example 2
[0056]
[0057]
[0058] In Table 2, TL is the liquidus temperature.
[0059] Table 2-3: Slag composition of Example 2
[0060]
[0061] (3) After demoulding, slice the ingot 200 mm from the bottom, and take two samples at the center, R / 2, and edge of the cross section for chemical composition testing. The results of chemical composition testing are shown in Table 2-4;
[0062] Table 2-4: Chemical composition test results of 1# to 3# electroslag ingots in Example 2 (wt%)
[0063]
[0064] Through organizational observation and chemical composition testing, the electroslag ingots obtained from 1# to 3# heats have qualified compositions, and the solidified structure and composition are uniform.
[0065] Embodiment 3:
[0066] (1) A 3t vacuum induction furnace and a 3t protective atmosphere electroslag furnace were used to carry out 3 furnaces of smelting, namely 1#, 2# and 3#. The target values of smelting composition are shown in Table 3-1;
[0067] Table 3-1: Chemical composition target of Example 3 (wt%)
[0068]
[0069] In Table 1, the balance is Fe and inevitable impurity elements.
[0070] (2) The vacuum smelting process: the casting ingot mold is Φ420×2900mm. The mass of the molten steel smelted in the vacuum furnace is 3000kg; the refining time is not less than Alloying time is not less than
[0071] The electroslag remelting process: Use a Φ530×2000mm crystallizer. The total mass of the pre-melted slag is 100kg, and the B2O3 content in the pre-melted slag is The amount of Al powder added is 100×(0.2~0.4)%=0.2kg~0.4kg. The melting rate is controlled to be (0.013~0.015)×D 结 =(0.013~0.015)×530=6.89kg / min~7.95kg / min.
[0072] The smelting process parameters of the 1# to 3# heats of this embodiment are shown in Table 3-2, and the slag components of the 1# to 3# heats are shown in Table 3-3;
[0073] Table 3-2: Smelting process parameters of Example 3
[0074]
[0075] In Table 2, TL is the liquidus temperature.
[0076] Table 3-3: Slag composition of Example 3
[0077]
[0078] (3) After demoulding, slice the electroslag ingot at a distance of 200 mm from the bottom, and take two samples at the center, R / 2, and edge of the cross section for chemical composition testing. The chemical composition test results are shown in Table 3-4;
[0079] Table 3-4: Chemical composition test results of 1# to 3# electroslag ingots in Example 3 (wt%)
[0080]
[0081]
[0082] Through organizational observation and chemical composition testing, the electroslag ingots obtained from 1# to 3# heats have qualified compositions, and the solidified structure and composition are uniform.
Claims
1. A method for smelting boron-containing steel for neutron shielding material, characterized in that: It includes vacuum smelting and electroslag remelting processes; The vacuum smelting process: refining time ≥√Mmin; after refining, 10000-30000Pa argon gas is charged into the furnace, and alloying is performed after the charging is completed, and the alloying time is ≥0.5×√Mmin; M is the mass of molten steel smelted in the vacuum furnace, kg; The electroslag remelting process: the slag system used is pre-melted slag and Al powder, the pre-melted slag contains B2O3; the content of B2O3 in the pre-melted slag [B2O3]% is determined according to the B content in the vacuum ingot, [B2O3]%=[(2.4×√a+3.3)]%, wherein a is the percentage of B in the vacuum ingot; the amount of Al powder added is 0.2% to 0.4% of the mass of the pre-melted slag.
2. The method for smelting boron-containing steel for neutron shielding material according to claim 1, characterized in that: In the electroslag remelting process, the pre-melted slag has the following components: CaF2 40%-47%, CaO 20%-25%, MgO 3%-5%, Al2O3 20%-25%, SiO2 4%-7% and B2O3.
3. The method for smelting boron-containing steel for neutron shielding material according to claim 1, characterized in that: In the vacuum smelting process, the tapping temperature of the molten steel is 40 to 60° C. above the liquidus.
4. A method for smelting boron-containing steel for neutron shielding material according to claim 1, 2 or 3, characterized in that: In the electroslag remelting process, the melting rate v is controlled to be (0.013-0.015)×D during the constant melting rate melting process. 结 , where v is the melting rate, kg / min, and D is the diameter of the electroslag furnace crystallizer, mm.
Citation Information
Patent Citations
High boron steel neutron absorbing material preparation method
CN101284306A
High-corrosion-resistance boron stainless steel material, preparation method and application
CN111826583A
Preparation method of boron stainless steel seamless tube for thermal neutron absorption
CN115921577A
Process method for improving yield of B and Nb in boron-containing heat-resistant steel
CN116121624A
Production of austenitic stainless steel for shielding neutron
JP1996215831A