Al2O3-based carrier monolithic catalyst with Ni-loaded TPMS structure as well as preparation method and application of Al2O3-based carrier monolithic catalyst

The preparation of Ni-supported TPMS-structured Al2O3-based monolithic catalysts using DLP technology solves the problems of high pressure drop, low heat and mass transfer efficiency, and difficulty in sample recovery of traditional powdered catalysts in fixed-bed reactors, achieving efficient catalyst recovery and reusability.

CN118925731APending Publication Date: 2024-11-12SHANGHAI INST OF TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411089837.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional powdered catalysts in fixed-bed continuous reactors suffer from problems such as high pressure drop, low heat and mass transfer efficiency, difficulty in sample recovery, and poor reusability.

Method used

A monolithic catalyst based on Al2O3 supported by a Ni-supported TPMS structure was prepared using digital light processing (DLP) technology. Catalysts with three-period minimal surface (TPMS) structures, including Diamond, IWP, Gyroid, and Pcell types, were prepared by 3D printing and ultrasonic impregnation.

Benefits of technology

A Ni-supported TPMS structure catalyst with high mass and heat transfer efficiency and easy recovery was achieved, exhibiting good reusability and improving the catalyst's stability and activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986216770000081
    Figure BDA0004986216770000081
  • Figure BDA0004986216770000091
    Figure BDA0004986216770000091
  • Figure HDA0004986216790000011
    Figure HDA0004986216790000011
Patent Text Reader

Abstract

The invention discloses an Al2O3-based carrier monolithic catalyst with a Ni-loaded TPMS structure as well as a preparation method and application of the Al2O3-based carrier monolithic catalyst, and the catalyst is prepared by adopting a digital light processing technology and has a three-period extremely small curved surface structure. The preparation process is simple, and the prepared Al2O3-based carrier monolithic catalyst with the Ni-loaded TPMS structure has the advantages that the mass transfer and heat transfer efficiency is high, a sample is easy to recover, and the reusability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of structural integral catalyst preparation, and specifically relates to an Al2O3-based carrier integral catalyst with a Ni-loaded TPMS structure, and a preparation method and application thereof. Background Art

[0002] Converting CO to synthetic natural gas (SNG) is of great significance for energy utilization and environmental protection. Transition metal Ni stands out among many methanation catalysts due to its low price and good methane selectivity. However, the high temperature during CO methanation easily causes the catalyst to be deactivated due to carbon deposition, so the preparation of high-temperature stable catalysts has become a major problem that needs to be solved in the industrial production of SNG.

[0003] In the prior art, traditional powder catalysts have disadvantages such as high pressure drop, low heat and mass transfer efficiency, difficulty in sample recovery, and poor reusability in fixed bed continuous reaction devices. Summary of the invention

[0004] The purpose of the present invention is to provide a Ni-loaded TPMS structure Al2O3-based carrier monolithic catalyst and its preparation method and application, so as to solve the problems of high pressure drop, low heat and mass transfer efficiency, difficult sample recovery and poor reusability of traditional powder catalysts in the prior art in a fixed bed continuous reaction device. The Ni-loaded TPMS structure Al2O3-based carrier monolithic catalyst prepared by the present invention has the advantages of high mass and heat transfer efficiency, easy sample recovery and good reusability.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] In one aspect, the present invention provides an Al2O3-based carrier monolithic catalyst with a Ni-loaded TPMS structure. The catalyst is prepared using digital light processing (DLP) technology and has a three-periodic minimal surface (TPMS) structure.

[0007] In another aspect, the present invention provides a method for preparing an Al2O3-based carrier monolithic catalyst having a Ni-supported TPMS structure, comprising the following steps:

[0008] (1) Carrier printing: using DLP 3D printing technology to print a TPMS structure Al2O3 carrier blank with a relative density of 20% to 50%, wherein the TPMS structure includes Diamond, IWP, Gyroid and Pcell structures;

[0009] (2) debinding and sintering: placing the green blank obtained in step (1) in a muffle furnace and heating the temperature to 1000°C to 1100°C at a rate of 0.2°C / min, maintaining the temperature, debinding, and sintering to obtain an Al2O3 carrier;

[0010] (3) Preparation of impregnation solution: Ni(NO3)2·6H2O is placed in a beaker, deionized water and anhydrous ethanol are added, and the mixture is fully dissolved to obtain an impregnation solution with a concentration of 10 to 50 wt%;

[0011] (4) Impregnation: placing the Al2O3 carrier of step (2) into the impregnation solution of step (3), and ultrasonically impregnating the carrier to obtain an Al2O3 structure loaded with Ni(NO3)2·6H2O;

[0012] (5) Drying: placing the structure of step (4) in an oven for drying to obtain a first precursor;

[0013] (6) Calcination: The first precursor of step (5) is placed in a muffle furnace and heated to 600-800° C. at 1° C. / min for calcination to obtain NiO / Al2O3, i.e., the second precursor;

[0014] (7) Reduction: The second precursor obtained in step (6) is placed in a fixed bed catalytic reactor, and H2 is introduced to carry out a reduction reaction to obtain a Ni / Al2O3 monolithic catalyst.

[0015] In step (2), the insulation time is 1 to 4 hours.

[0016] In step (3), the impregnation amount of Ni(NO3)2·6H2O is 1-10wt% of the Al2O3 carrier.

[0017] In step (3), the volume ratio of deionized water to anhydrous ethanol is 1:1.

[0018] In step (4), the immersion time is 1 to 4 hours.

[0019] In step (5), the temperature of the drying treatment is 100-200° C., and the time of the drying treatment is 12 hours.

[0020] In step (7), the temperature of the reduction reaction is 400-500°C; preferably, the temperature of the reduction reaction is 480°C.

[0021] In a third aspect, the present invention further provides the use of the above-mentioned Ni-loaded TPMS structured Al2O3-based carrier monolithic catalyst, or a catalyst prepared according to the above-mentioned method for preparing the Ni-loaded TPMS structured Al2O3-based carrier monolithic catalyst in CO methanation.

[0022] The positive and progressive effects of the present invention are:

[0023] The present invention uses 3D printing technology and ultrasonic impregnation method to prepare TPMS structure catalysts with a relative density of 20% to 50%, including Gyroid, Diamond, Pcell and IWP structures. The preparation process of the present invention is simple, and the prepared Al2O3-based carrier monolithic catalyst with Ni-loaded TPMS structure has the advantages of high mass and heat transfer efficiency, easy sample recovery, and good reusability. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Creo software design drawing models and physical pictures of four integral catalysts with TPMS structure designed and prepared by the present invention; wherein, Figure a is the design drawing model of Diamond type, Figure b is the physical picture of Diamond type, Figure c is the design drawing model of Gyroid type, Figure d is the physical picture of Gyroid, Figure e is the design drawing model of IWP type, Figure f is the physical picture of IWP, Figure g is the design drawing model of Pcell type, and Figure h is the physical picture of Pcell;

[0025] Figure 2 This is a test diagram of the reusability of the catalysts prepared in Examples 1 to 4 of the present invention;

[0026] Figure 3 This is a physical comparison diagram of the catalysts prepared in Comparative Example 3 (left) and Example 6 (right) of the present invention. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with the embodiments, and the technical scheme of the present invention is clearly and completely described to facilitate the understanding of the present invention by those skilled in the art. The described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products; the process steps or preparation methods not mentioned in detail are process steps or preparation methods known to those skilled in the art.

[0028] Example 1

[0029] (1) Carrier printing: Using a DLP printer to print out the designed Al2O3 with a TPMS structure of 30% relative density, obtaining an Al2O3 blank with a diamond-type structure;

[0030] (2) Debinding and sintering: The green blank obtained in step (1) was placed in a muffle furnace, and the temperature was raised to 1050° C. at a rate of 0.2° C. / min, and kept at this temperature for 2 h to perform debinding and sintering treatments to obtain an Al2O3 carrier;

[0031] (3) Preparation of impregnation solution: Weigh 2.57 g of Ni(NO3)2·6H2O into a beaker, add 20 mL of deionized water and anhydrous ethanol in a volume ratio of 1:1 to dissolve, and obtain an impregnation solution with a concentration of 12 wt%;

[0032] (4) Impregnation: placing the support obtained in step (2) into the impregnation solution obtained in step (3), and ultrasonically impregnating the support in an ultrasonic cleaning apparatus for 1 h to obtain an Al2O3 structure loaded with Ni(NO3)2·6H2O;

[0033] (5) Drying: The structure obtained in step (4) is placed in an oven at 100° C. for 12 h to remove surface moisture, thereby obtaining a first precursor;

[0034] (6) Calcination: The first precursor obtained in step (5) is placed in a muffle furnace and heated to 700° C. at 1° C. / min for calcination to obtain NiO / Al2O3, i.e., the second precursor;

[0035] (7) Reduction: The second precursor obtained in step (6) is placed in a fixed bed catalytic reactor, and 50 mL / min of 99.9% pure H2 is introduced at 480°C and normal pressure for a reduction reaction for 3 h to obtain a Ni / Al2O3 monolithic catalyst.

[0036] Example 2

[0037] The only difference from Example 1 is that the structure of the Al2O3 blank in step (1) is of Gyroid type.

[0038] Example 3

[0039] The only difference from Example 1 is that the structure of the Al2O3 blank in step (1) is of IWP type.

[0040] Example 4

[0041] The only difference from Example 1 is that the structure of the Al2O3 blank in step (1) is of Pcell type.

[0042] Example 5

[0043] (1) Carrier printing: Using a DLP printer to print out the designed TPMS structure of Al2O3 with a relative density of 30%, a Gyroid-type Al2O3 blank is obtained;

[0044] (2) Debinding and sintering: The green blank obtained in step (1) was placed in a muffle furnace, and the temperature was raised to 1000° C. at a rate of 0.2° C. / min, and kept at that temperature for 1 h to perform debinding and sintering treatments to obtain an Al2O3 carrier;

[0045] (3) Preparation of impregnation solution: Weigh 2.57 g of Ni(NO3)2·6H2O into a beaker, add 20 mL of deionized water and anhydrous ethanol in a volume ratio of 1:1 to dissolve, and obtain an impregnation solution with a concentration of 12 wt%;

[0046] (4) Impregnation: placing the support obtained in step (2) into the impregnation solution obtained in step (3), and ultrasonically impregnating the support in an ultrasonic cleaning apparatus for 2 h to obtain an Al2O3 structure loaded with Ni(NO3)2·6H2O;

[0047] (5) Drying: The structure obtained in step (4) is placed in an oven at 110° C. and dried for 12 h to remove surface moisture, thereby obtaining a first precursor;

[0048] (6) Calcination: The first precursor obtained in step (5) is placed in a muffle furnace and heated to 600° C. at 1° C. / min for calcination to obtain NiO / Al2O3, i.e., the second precursor;

[0049] (7) Reduction: The second precursor obtained in step (6) is placed in a fixed bed catalytic reactor, and 50 mL / min of 99.9% pure H2 is introduced at 480°C and normal pressure for a reduction reaction for 3 h to obtain a Ni / Al2O3 monolithic catalyst.

[0050] Example 6

[0051] (1) Carrier printing: Using a DLP printer to print out the designed TPMS structure of Al2O3 with a relative density of 30%, a Gyroid-type Al2O3 blank is obtained;

[0052] (2) Debinding and sintering: The green blank obtained in step (1) was placed in a muffle furnace, and the temperature was raised to 1100° C. at a rate of 0.2° C. / min, and kept at this temperature for 4 h to perform debinding and sintering treatments to obtain an Al2O3 carrier;

[0053] (3) Preparation of impregnation solution: Weigh 2.57 g of Ni(NO3)2·6H2O into a beaker, add 20 mL of deionized water and anhydrous ethanol in a volume ratio of 1:1 to dissolve, and obtain an impregnation solution with a concentration of 12 wt%;

[0054] (4) Impregnation: placing the support obtained in step (2) into the impregnation solution obtained in step (3), and ultrasonically impregnating the support in an ultrasonic cleaning apparatus for 4 h to obtain an Al2O3 structure loaded with Ni(NO3)2·6H2O;

[0055] (5) Drying: The structure obtained in step (4) is placed in an oven at 200° C. for 12 h to remove surface moisture, thereby obtaining a first precursor;

[0056] (6) Calcination: The first precursor obtained in step (5) is placed in a muffle furnace and heated to 800° C. at 1° C. / min for calcination to obtain NiO / Al2O3, i.e., the second precursor;

[0057] (7) Reduction: The second precursor obtained in step (6) is placed in a fixed bed catalytic reactor, and 50 mL / min of 99.9% pure H2 is introduced at 480°C and normal pressure for a reduction reaction for 3 h to obtain a Ni / Al2O3 monolithic catalyst.

[0058] Example 7

[0059] The only difference from Example 6 is that the relative density in step (1) is 20%.

[0060] Example 8

[0061] The only difference from Example 6 is that the relative density in step (1) is 40%.

[0062] Example 9

[0063] The only difference from Example 6 is that the relative density in step (1) is 50%.

[0064] Example 10

[0065] The only difference from Example 6 is that in step (3), the weighed amount of Ni(NO3)2·6H2O is 7.67 g and the concentration of the impregnation solution is 30 wt%.

[0066] Embodiment 11

[0067] The only difference from Example 6 is that in step (3), the weighed amount of Ni(NO3)2·6H2O is 12.18 g and the concentration of the impregnation solution is 40 wt%.

[0068] Example 12

[0069] The only difference from Example 6 is that in step (3), the weighed amount of Ni(NO3)2·6H2O is 17.01 g and the concentration of the impregnation solution is 48 wt%.

[0070] Comparative Example 1

[0071] The commercially purchased Al2O3 powder of model 012a produced by Jiaxing Raoji Technology Co., Ltd. (the powder in the 3D printing slurry) was prepared into a Ni / Al2O3 powder catalyst according to the above method and placed in a fixed bed catalytic reactor. 50 mL / min of H2 with a purity of 99.9% was introduced at 480°C and normal pressure for a reduction reaction. The reduction time was 3 hours to obtain a powdered Ni / Al2O3 catalyst.

[0072] Comparative Example 2

[0073] The only difference from Example 6 is that in step (3), 2.57 g of Ni(NO3)2·6H2O is weighed into a beaker, and 20 mL of anhydrous ethanol is added to dissolve it to obtain an impregnation solution with a concentration of 12 wt%.

[0074] Comparative Example 3

[0075] The only difference from Example 6 is that the impregnation method in step (4) is: the carrier obtained in step (2) is directly immersed in the impregnation solution obtained in step (3) without using an ultrasonic cleaner.

[0076] Comparative Example 4

[0077] The only difference from Example 6 is that the calcination temperature in step (6) is 200°C.

[0078] Effect Example

[0079] The following performance tests were performed on the products of Examples 1 to 12 and Comparative Examples 1 to 4 of the present application:

[0080] 1. Catalytic reaction test: The catalyst was heated at 480°C, and a reaction gas with a ratio of CO and H2 of 1:3 was introduced. The back pressure valve was adjusted to make the reaction pressure reach 1MPa. The reaction was carried out for 8 hours, and the product was analyzed by gas chromatography.

[0081] 2. Reusability test (repeatability test means repeating the reduction test for 8 hours every day and observing the catalyst until it is deactivated): (1) Place the catalyst in a fixed bed catalytic reactor and reduce it with hydrogen at 480℃ for 3 hours. Then, introduce a reaction gas with a ratio of CO and H2 of 1:3. Adjust the back pressure valve so that the reaction pressure reaches 1MPa and the reaction temperature is 480℃. Stop the reaction after 8 hours and wait for the temperature to cool to room temperature.

[0082] (2) On the next day, the catalyst was reduced again under the above conditions for 3 h, and the reaction was repeated under the above reaction conditions for 8 h, and the product was analyzed by gas chromatography until the catalyst lost its reactivity.

[0083] (3) The CO conversion rates after 2 h of reaction at different days were compared to test the reusability of the catalyst.

[0084] The performance tests were carried out on the catalysts prepared in Examples 1 to 12 and Comparative Examples 1 to 4. The results are shown in Table 1.

[0085] Table 1

[0086]

[0087]

[0088] from Figure 1 It can be seen that four different catalysts with different TPMS structural channels were successfully prepared.

[0089] Based on the catalyst catalytic activity test, the reusability test results of the four monolithic catalysts are as follows: Figure 2 As shown, the results show that Diamond and Gyroid catalysts not only have good catalytic performance, but also after 6 days of reusability test, their CO conversion rate remains above 90%, showing excellent stability. The main reason is that the Diamond and Gyroid structures have better heat transfer performance and can effectively avoid local temperature rise caused by uneven heat transfer during the reaction to produce high-temperature hotspots, thereby causing catalyst deactivation.

[0090] Examples 6 to 9 are monolithic catalysts with different relative densities. The catalytic activity of the catalysts prepared in Examples 6 to 9 was tested. As can be seen from Table 1, the catalytic activity of the monolithic catalysts with different relative densities is also good, and the conversion rate is above 98.7% after 8 hours of reaction.

[0091] Examples 6, 10 to 12 are monolithic catalysts with different impregnation amounts. The catalytic activities of the catalysts prepared in Examples 6, 10 to 12 were compared. As can be seen from Table 1, the catalytic activities of the monolithic catalysts at different loading amounts are all very good, and the conversion rates after 8 hours of reaction are all above 98.7%.

[0092] Figure 3 This is a physical comparison diagram of the catalyst prepared in Comparative Example 3 (left) and Example 6 (right) of the present invention. Figure 3 It can be seen that the catalyst in Comparative Example 3 is not evenly impregnated after reduction, which is due to the heat generated during the ultrasonic vibration and the volatilization of part of the anhydrous ethanol. The CO conversion rate of the catalyst prepared in Comparative Example 3 is only 85%.

[0093] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and equivalent changes made by using the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. An Al2O3-based carrier monolithic catalyst with a Ni-supported TPMS structure, characterized in that: The catalyst is prepared by adopting digital light processing technology and has a three-periodic minimal surface structure.

2. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 1, characterized in that: The following steps are involved: (1) Carrier printing: using DLP 3D printing technology to print a TPMS structure Al2O3 carrier blank with a relative density of 20% to 50%, wherein the TPMS structure includes Diamond, IWP, Gyroid and Pcell structures; (2) debinding and sintering: placing the green blank obtained in step (1) in a muffle furnace and heating the temperature to 1000°C to 1100°C at a rate of 0.2°C / min, maintaining the temperature, debinding, and sintering to obtain an Al2O3 carrier; (3) Preparation of impregnation solution: Ni(NO3)2·6H2O is placed in a beaker, and deionized water and anhydrous ethanol are added to fully dissolve to obtain an impregnation solution with a concentration of 10 to 50 wt%; (4) Impregnation: placing the Al2O3 carrier of step (2) into the impregnation solution of step (3), and ultrasonically impregnating the carrier to obtain an Al2O3 structure loaded with Ni(NO3)2·6H2O; (5) Drying: placing the structure of step (4) in an oven for drying to obtain a first precursor; (6) Calcination: The first precursor of step (5) is placed in a muffle furnace and heated to 600-800° C. at 1° C. / min for calcination to obtain NiO / Al2O3, i.e., the second precursor; (7) Reduction: The second precursor obtained in step (6) is placed in a fixed bed catalytic reactor, and H2 is introduced to carry out a reduction reaction to obtain a Ni / Al2O3 monolithic catalyst.

3. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 2, characterized in that: In step (2), the insulation time is 1 to 4 hours.

4. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 2, characterized in that: In step (3), the impregnation amount of Ni(NO3)2·6H2O is 1-10wt% of the Al2O3 carrier.

5. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 2, characterized in that: In step (3), the volume ratio of deionized water to anhydrous ethanol is 1:

1.

6. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 2, characterized in that: In step (4), the immersion time is 1 to 4 hours.

7. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 2, characterized in that: In step (5), the temperature of the drying treatment is 100-200° C., and the time of the drying treatment is 12 hours.

8. The method for preparing the Al2O3-based carrier monolithic catalyst with Ni-supported TPMS structure according to claim 2, characterized in that: In step (7), the temperature of the reduction reaction is 400-500°C; preferably, the temperature of the reduction reaction is 480°C.

9. Use of the Al2O3-based carrier monolithic catalyst with a Ni-supported TPMS structure according to claim 1, or the catalyst prepared according to the preparation method of the Al2O3-based carrier monolithic catalyst with a Ni-supported TPMS structure according to claims 2 to 8 in CO methanation.

Citation Information

Cited By

  • Aluminum oxide catalyst with metal monatomic supported bionic bicontinuous amplitude-modulated decomposition structure as well as preparation method and application of aluminum oxide catalyst

    CN120079372A

  • Alumina catalyst with metal single-atom supported biomimetic bicontinuous amplitude modulation decomposition structure, and preparation method and application thereof

    CN120079372B

  • Metal monatomic supported aluminum oxide ceramic dot matrix catalyst as well as preparation method and application thereof

    CN120285972A