Preparation method of ferromanganese phosphate, ferromanganese phosphate, positive electrode material and battery

By using a segmented feed method of complexing agent and oxidizing agent in the preparation of ferromanganese phosphate, the problems of toxic substances and precipitation uniformity in the prior art are solved, and safe and environmentally friendly preparation and industrial applicability of ferromanganese phosphate are achieved.

CN118929612AActive Publication Date: 2024-11-12JINCHI ENERGY MATERIALS CO LTD +2

Patent Information

Application Number
CN202411160706.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The existing preparation methods for ferromanganese phosphate use toxic cyanide and strong oxidizing agents, which pose safety risks and are not suitable for industrial applications, and the uniform precipitation effect of iron and manganese is not good.

Method used

采用在锰源、铁源、磷源的混合溶液中加入络合剂和氧化剂,通过分段调节pH值和温度,进行固液分离和煅烧,制备出磷酸锰铁,实现铁锰的均匀沉淀和内外层结构的控制。

Benefits of technology

It realizes safe and environmentally friendly preparation of ferromanganese phosphate, with simple process and high operability, and uniform distribution of iron and manganese, loose and porous inner layer and dense outer layer, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929612A_ABST
    Figure CN118929612A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of battery materials, and mainly discloses a preparation method of ferromanganese phosphate, which comprises the following steps: S1, adding a complexing agent and an oxidizing agent into a mixed solution A of a manganese source, an iron source and a phosphorus source to obtain a mixed solution B; s2, dividing the mixed solution B into a mixed solution B-1 and a mixed solution B-2; s3, adjusting the pH value of the mixed solution B-1 to 2.0-5.0, heating the mixed solution B-1 to 90-100 DEG C, and keeping the temperature to obtain slurry I; step S4, adding the mixed solution B-2 into the slurry I, adjusting the pH value of the system to 1-5, and keeping the temperature at 60-100 DEG C to obtain slurry II; and S5, carrying out solid-liquid separation, drying, screening and calcining on the slurry II to obtain a solid phase, namely the ferromanganese phosphate. In the process of preparing ferromanganese phosphate, toxic and harmful reagents are not used, safety and environmental protection are achieved, and industrial application is facilitated; and the prepared ferromanganese phosphate has a loose and porous inner layer and a dense and compact outer layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of battery materials and specifically discloses ferromanganese phosphate and a preparation method and application thereof. Background Art

[0002] Lithium iron manganese phosphate material is a battery positive electrode material that not only inherits the safety and stability of lithium iron phosphate, but also has the advantages of higher energy density, lower cost and longer life. The precursor material of lithium iron manganese phosphate material is iron manganese phosphate material.

[0003] CN115321507A discloses a method for preparing ferromanganese phosphate by coprecipitation, respectively preparing ferrocyanide solution, manganese salt solution and a mixed solution of phosphoric acid and perchloric acid, adding ferrocyanide solution, manganese salt solution, mixed solution and alkali solution to the bottom liquid and reacting, when the reaction mass reaches the target particle size, solid-liquid separation is carried out to obtain a precipitate, and the precipitate is washed and dried to obtain ferromanganese phosphate. Ferrocyanide is utilized to suppress the direct precipitation of trivalent iron ions, perchloric acid and phosphoric acid are used to carry out cyanide breaking reaction, the precipitation rate of ferromanganese phosphate is slowed down, iron manganese is made to reach coprecipitation, and the uniformity of iron manganese mixing is improved. However, poisonous cyanide and strong oxidant perchloric acid are used, which is not suitable for industrial application. Summary of the invention

[0004] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a method for preparing ferromanganese phosphate which is safe, environmentally friendly and has uniform precipitation of iron and manganese; the second purpose of the present invention is to provide ferromanganese phosphate and its application.

[0005] In order to solve the above problems, the present invention proposes the following specific technical solutions.

[0006] First, the present invention provides a method for preparing ferromanganese phosphate, comprising: Step S1, adding a complexing agent and an oxidant to a mixed solution A of a manganese source, an iron source, and a phosphorus source to obtain a mixed solution B; Step S2, dividing the mixed solution B into two parts, a mixed solution B-1 and a mixed solution B-2; Step S3, adjusting the pH value of the mixed solution B-1 to 2.0-5.0, heating to 90-100° C., and keeping the temperature to obtain slurry I; Step S4, adding the mixed solution B-2 to the slurry I, adjusting the pH value of the system to 1-5, and keeping the temperature at 60-100° C. to obtain slurry II; Step S5, separating the slurry II into solid and liquid, drying, screening and calcining the obtained solid phase to obtain ferromanganese phosphate.

[0007] In a further preferred embodiment, the total molar concentration of manganese and iron in the mixed solution A is 0.2-2.0 mol / L.

[0008] In a further preferred embodiment, the molar ratio of manganese to iron in the mixed solution A is 1-2:1.

[0009] In a further preferred embodiment, the ratio of the molar amount of the complexing agent to the total molar amount of iron and manganese is 1-2:1.

[0010] In a further preferred embodiment, the ratio of the molar amount of the oxidant to the total molar amount of iron and manganese is 1-1.5:1.

[0011] In a further preferred embodiment, the manganese source is at least one of manganese sulfate, manganese nitrate, manganese chloride, manganese oxalate, and manganese acetate; the iron source is at least one of ferrous sulfate, ferrous nitrate, ferrous chloride, ferrous oxalate, and ferrous acetate; the phosphorus source is at least one of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium phosphate; the chelating agent is sodium pyrophosphate, potassium pyrophosphate, phosphoric acid, diammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, DFOB, iron-free feces The oxidant is at least one of hydrogen peroxide, ammonium persulfate, sodium persulfate, potassium persulfate, ozone, nitric acid, ammonium nitrate, potassium nitrate, sodium nitrate, potassium permanganate, dichromic acid, chlorine, chloric acid, hypochlorous acid, chlorous acid, perchloric acid, hypoiodous acid, metaperiodic acid, bromic acid, hypobromous acid, perbromic acid, ferrate, and fluorine.

[0012] In a further preferred embodiment, the volume ratio of the mixed solution B-1 to the mixed solution B-2 is (20-40): (80-60).

[0013] In a further preferred embodiment, in step S3, the pH value of the mixed solution B-1 is adjusted to 3.0-5.0.

[0014] In a further preferred embodiment, in step S3, the temperature is heated to 95-100°C.

[0015] In a further preferred embodiment, in step S3, the insulation time is 1 to 2 hours.

[0016] In a further preferred embodiment, in step S4, the pH value of the system is adjusted to 1.5-3.0.

[0017] In a further preferred embodiment, in step S4, the temperature is kept at 80-95°C.

[0018] In a further preferred embodiment, in step S4, the insulation time is 0.5 to 2 hours.

[0019] In a further preferred embodiment, in step S5, the drying temperature is 90-150°C; and the calcining temperature is 200-600°C.

[0020] In a further preferred embodiment, stirring is performed during step S1, step S3 and step S4; and further preferably, the stirring speed is 100-1000 rpm.

[0021] Secondly, the present invention provides a manganese iron phosphate, the chemical formula of which is Mn x Fe 1-x PO4, wherein 0.1≤x≤0.9, preferably 0.4≤x≤0.8; is a secondary particle formed by agglomeration of primary particles, and has a spherical or quasi-spherical structure; comprises an inner core and an outer shell, wherein the inner core is loose and porous, and the outer shell is relatively compact.

[0022] In a further preferred embodiment, the diameter of the primary particles of the shell is 75-500 nm; the diameter of the primary particles of the core is smaller than the diameter of the primary particles of the shell.

[0023] In a further preferred embodiment, the ratio of the thickness of the outer shell to the radius of the inner core is 0.8-3.0:1.

[0024] In a further preferred embodiment, the ferromanganese phosphate satisfies at least one of the following conditions (a) to (c): (a) the porosity of the inner core is 30-60%, preferably 40-50%; (b) The porosity of the shell is 0.01-5%, preferably 0.05-2%; (c) The porosity difference between the inner core and the outer shell is 25-60%, preferably 40-50%.

[0025] In a further preferred embodiment, the ferromanganese phosphate satisfies at least one of the following conditions (d) to (f): (d) the primary particles constituting the shell are in the shape of dendrites or strips; (e) the average aspect ratio of the primary particles constituting the shell is 1.0 to 4.0, preferably 1.5 to 3.0; (f) The particle size D50 of the secondary particles is 5.0-9.0 μm.

[0026] Based on the same inventive concept, the ferromanganese phosphate provided by the present invention can be prepared by the aforementioned preparation method.

[0027] In addition, the present invention provides a positive electrode material prepared from the above-mentioned ferromanganese phosphate, and provides a battery comprising the positive electrode material.

[0028] The above one or more technical solutions of the present invention can achieve at least one of the following beneficial effects: The preparation method provided by the invention has simple process and high operability.

[0029] In the process of preparing ferromanganese phosphate, no toxic or harmful reagents are used, the process is safe, environmentally friendly and conducive to industrial application.

[0030] The preparation method provided by the invention can make MnPO4 and FePO4 co-precipitate at the same time, and the iron and manganese are evenly distributed.

[0031] The ferromanganese phosphate provided by the invention has a loose and porous inner layer and a dense and compact outer layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 1.

[0033] Figure 2 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 1.

[0034] Figure 3 This is the SEM image of the ferromanganese phosphate material obtained in Example 1.

[0035] Figure 4 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 1.

[0036] Figure 5 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 2.

[0037] Figure 6 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 2.

[0038] Figure 7 This is the SEM image of the ferromanganese phosphate material obtained in Example 2.

[0039] Figure 8 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 2.

[0040] Fig. 9 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 3.

[0041] Fig.10 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 3.

[0042] Fig.11 This is the SEM image of the ferromanganese phosphate material obtained in Example 3.

[0043] Fig.12 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 3.

[0044] Fig.13This is the XRD diagram of the ferromanganese phosphate material obtained in Example 4.

[0045] Fig.14 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 4.

[0046] Fig.15 This is the SEM image of the ferromanganese phosphate material obtained in Example 4.

[0047] Fig.16 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 4.

[0048] Fig.17 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 5.

[0049] Fig.18 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 5.

[0050] Fig.19 This is the SEM image of the ferromanganese phosphate material obtained in Example 5 Fig. 20 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 5.

[0051] Fig.21 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 6.

[0052] Fig. 22 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 6.

[0053] Fig.23 This is the SEM image of the ferromanganese phosphate material obtained in Example 6.

[0054] Fig.24 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 6.

[0055] Fig.25 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 1.

[0056] Fig.26 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 1.

[0057] Fig. 27 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 1.

[0058] Fig.28 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 1.

[0059] Fig.29 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 2.

[0060] Fig.30 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 2.

[0061] Fig.31 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 2.

[0062] Fig.32 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 2.

[0063] Fig.33 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 3.

[0064] Fig.34 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 3.

[0065] Fig.35 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 3.

[0066] Fig.36 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 3.

[0067] Fig.37 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 4.

[0068] Fig.38 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 4.

[0069] Fig.39 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 4.

[0070] Fig.40 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 4.

[0071] Fig.41 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 5.

[0072] Fig.42 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 6.

[0073] Fig.43 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 7.

[0074] Fig.44 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 8.

[0075] Fig.45 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 9.

[0076] Fig.46 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 10.

[0077] Fig.47 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 11. DETAILED DESCRIPTION

[0078] First, the present invention provides a method for preparing ferromanganese phosphate, comprising the following steps: Step S1, adding a complexing agent and an oxidant to a mixed solution A of a manganese source, an iron source, and a phosphorus source to obtain a mixed solution B; Step S2, dividing the mixed solution B into two parts, a mixed solution B-1 and a mixed solution B-2; Step S3, adjusting the pH value of the mixed solution B-1 to 2.0-5.0, heating to 90-100° C., and keeping the temperature to obtain slurry I; Step S4, adding the mixed solution B-2 to the slurry I, adjusting the pH value of the system to 1-5, and keeping the temperature at 60-100° C. to obtain slurry II; Step S5, separating the slurry II into solid and liquid, drying, screening and calcining the obtained solid phase to obtain ferromanganese phosphate.

[0079] In specific practice, the contents of manganese source, iron source and phosphorus source in the mixed solution A are set according to the ratio of manganese, iron and phosphorus in the target manganese ferrophosphate. x Fe 1-x PO4 (wherein 0.1≤x≤0.9, preferably 0.4≤x≤0.8) determines the contents of the manganese source, iron source and phosphorus source in the mixed solution A.

[0080] In some embodiments of the present invention, the total molar concentration of manganese and iron in the mixed solution A is 0.2-2.0 mol / L. It is further preferred that the molar ratio of manganese to iron in the mixed solution A is 1-2:1.

[0081] In specific practice, those skilled in the art can select appropriate manganese source, iron source and phosphorus source according to actual conditions. Generally speaking, they can be dissolved in water. In a specific embodiment of the present invention: The manganese source is at least one of manganese sulfate, manganese nitrate, manganese chloride, manganese oxalate, and manganese acetate; The iron source is at least one of ferrous sulfate, ferrous nitrate, ferrous chloride, ferrous oxalate, and ferrous acetate; The phosphorus source is at least one of phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, ammonium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, and sodium phosphate.

[0082] In the present invention, the oxidant and the complexing agent are used in combination to stabilize the manganese in the solution in a trivalent state. In addition, as for the amount of the complexing agent and the oxidant used, the principle of "stabilizing the manganese in the solution in a trivalent state" should also be followed. Based on the principle, those skilled in the art adjust the amount of the complexing agent and the oxidant according to actual conditions.

[0083] In a specific embodiment of the present invention, the ratio of the molar amount of the complexing agent to the total molar amount of iron and manganese is 1-2:1; the ratio of the molar amount of the oxidant to the total molar amount of iron and manganese is 1-1.5:1. In the present invention, when the amount of the complexing agent is too high, the preparation cost increases significantly; when the amount of the complexing agent is too low, incomplete complexation may cause partial Mn 3+ Disproportionate to Mn 2+ With Mn 4+ ; When the oxidant dosage is too high, Mn may exist 4+ When the amount of oxidant is too low, incomplete oxidation will occur.

[0084] For those skilled in the art, any complexing agent that can play a complexing role and is common in the art can achieve the purpose of the present invention. In a specific embodiment of the present invention, the complexing agent is at least one of sodium pyrophosphate, potassium pyrophosphate, phosphoric acid, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium phosphate, DFOB, desferrioxan, acetohydroxyamine, 2,5-diacylhydroxamic acid, 3,4-diacylhydroxamic acid, EDTA, disodium EDTA, sodium citrate, ammonium citrate, and potassium citrate.

[0085] It should be emphasized that phosphoric acid is further selected as a complexing agent in the preferred embodiment of the present invention. Phosphoric acid can be used as both a phosphorus source and a complexing agent in the present invention, and phosphoric acid can also be used as a pH adjuster in the present invention.

[0086] The oxidant is a common chemical in the art. In a specific embodiment of the present invention, the oxidant is at least one of hydrogen peroxide, ammonium persulfate, sodium persulfate, potassium persulfate, ozone, nitric acid, ammonium nitrate, potassium nitrate, sodium nitrate, potassium permanganate, dichromic acid, chlorine, chloric acid, hypochlorous acid, chlorous acid, perchloric acid, hypoiodous acid, metaperiodic acid, bromic acid, hypobromous acid, perbromic acid, ferrate, and fluorine. It is further preferred that the oxidant is ammonium persulfate.

[0087] Step S3 and step S4 are also the key to the present invention. By means of segmented feeding synthesis, the supersaturation of the reaction system is controlled, the crystal nucleation and growth process is regulated, and the manganese iron phosphate material is prepared. At the same time, segmented feeding is adopted, and the thickness or proportion of the inner and outer layers is controlled by the amount of the front and rear solutions. The temperature of the synthesis process, the pH value of the system, etc. are controlled to obtain a manganese iron phosphate material with a porous inner layer and a dense outer layer. On the basis of step S1 (through the interaction of the oxidant and the complexing agent, Mn3+ Stable in solution), regulate the pH value and reaction temperature during precipitation, and thus control the Mn 3+ , Fe 3+ The precipitation efficiency of Mn 3+ , Fe 3+ The pH value and temperature affect the supersaturation of the solution in the reaction system. Supersaturation directly affects the nucleation and growth process. When the supersaturation is high, nucleation is dominant; when the supersaturation is low, growth is dominant. In order to achieve a loose interior and a dense shell, the reaction is regulated to be dominated by nucleation in the early stage and growth in the later stage. In addition, the thickness of the inner core and the outer shell can also be controlled by regulating the time of nucleation and growth.

[0088] In a specific embodiment of the present invention, the volume ratio of the mixed solution B-1 to the mixed solution B-2 is (20-40): (80-60), and more preferably 40:60, 30:70, or 20:80.

[0089] In a preferred embodiment of the present invention, in step S3, the pH value of the mixed solution B-1 is adjusted to 3.0-5.0, more preferably 3.0, 3.5, 4.0, 5.0.

[0090] In a preferred embodiment of the present invention, in step S3, heating is performed to 95-100°C.

[0091] In a preferred embodiment of the present invention, in step S3, the insulation time is 1 to 2 hours.

[0092] In a preferred embodiment of the present invention, in step S4, the pH value of the system is adjusted to 1.5-3.0, more preferably 1.5, 2.0, 2.7, 3.0.

[0093] In a preferred embodiment of the present invention, in step S4, the temperature is kept at 80-95°C, more preferably 80°C, 85°C, 90°C, 95°C.

[0094] In a preferred embodiment of the present invention, in step S4, the insulation time is 0.5-2h.

[0095] In some embodiments of the present invention, in step S5, the drying temperature is 90-150°C, and more preferably 90°C, 100°C, 120°C, and 150°C; the calcination temperature is 200-600°C, and more preferably 450°C, 480°C, 500°C, and 550°C.

[0096] In a preferred embodiment of the present invention, stirring is performed during step S1, step S3 and step S4; further preferably, the stirring speed is 100-1000 rpm, and more preferably, the stirring speed is 350 rpm, 500 rpm, 800 rpm, or 1000 rpm.

[0097] Secondly, the present invention provides a manganese iron phosphate, the chemical formula of which is Mn x Fe 1-x PO4, wherein 0.1≤x≤0.9, preferably 0.4≤x≤0.8, for example, x is 0.5, 0.6, 0.7; and ferromanganese phosphate is a secondary particle formed by agglomeration of primary particles, and has a spherical or quasi-spherical structure; it includes an inner core and an outer shell, the inner core is loose and porous, and the outer shell is relatively compact.

[0098] The inner core of the ferromanganese phosphate material is loose and porous, which is conducive to the diffusion of lithium into the interior of the material during the subsequent sintering process of the positive electrode material; the relatively compact outer shell is conducive to achieving a higher tap density, improving the crystallization integrity of the positive electrode material after sintering, and greatly reducing the ferromanganese dissolution rate of the positive electrode material.

[0099] In a preferred embodiment of the present invention, the diameter of the primary particles of the shell is 75-500 nm, for example, 78 nm, 123 nm, 195 nm, 203 nm, 250 nm, 470 nm; the diameter of the primary particles of the core is smaller than the diameter of the primary particles of the shell. The primary particles of the core and the shell have different diameters, so that the prepared positive electrode material spontaneously produces a grading effect, thereby increasing the compaction density of the positive electrode material.

[0100] In a preferred embodiment of the present invention, the ratio of the thickness of the outer shell to the radius of the inner core is 0.8-3.0:1, for example, it can be 0.84, 1.32, 1.42, 1.51, 1.68, or 2.70.

[0101] In a preferred embodiment of the present invention, the ferromanganese phosphate satisfies at least one of the following conditions (a) to (c): (a) the porosity of the inner core is 30-60%, preferably 40-50%; (b) The porosity of the shell is 0.01-5%, preferably 0.05-2%; (c) The porosity difference between the inner core and the outer shell is 25-60%, preferably 40-50%.

[0102] In a preferred embodiment of the present invention, the ferromanganese phosphate satisfies at least one of the following conditions (d) to (f): (d) the primary particles constituting the shell are in the shape of dendrites or strips; (e) the average aspect ratio of the primary particles constituting the shell is 1.0 to 4.0, preferably 1.5 to 3.0; (f) The particle size D50 of the secondary particles is 5.0-9.0 μm.

[0103] It is further explained that the average aspect ratio of the primary particles in the present invention refers to the ratio of the length from the visible root of the primary particle to the vertex of the primary particle to the maximum width of the primary particle.

[0104] Based on the same inventive concept, the ferromanganese phosphate provided by the present invention can be prepared by the aforementioned preparation method.

[0105] In addition, the present invention provides a positive electrode material prepared from the above-mentioned ferromanganese phosphate, and provides a battery comprising the positive electrode material.

[0106] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0107] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0108] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0109] In the specific embodiments and comparative examples, the main testing methods include: XRD test: Japan Rigaku SmartLab SE intelligent X-ray diffractometer.

[0110] SEM test: Japan field emission scanning electron microscope.

[0111] EDS test: EDAX energy spectrometer.

[0112] Porosity: The analysis software used was Image J, and the porosity was calculated as follows: porosity = pore area of ​​each region / cross-sectional area of ​​each region × 100%.

[0113] Primary particle size: measured using NanoMeasurer software.

[0114] Example 1 (1) According to the chemical formula Mn 0.6 Fe 0.4 PO4, add manganese sulfate and ferrous sulfate to a certain amount of pure water, stir until the solution is clear, add phosphoric acid solution in an equal molar amount to manganese sulfate and ferrous sulfate, stir thoroughly, and then add an appropriate amount of pure water to make up the volume. Finally, a mixed solution A with a manganese sulfate concentration of 0.9 mol / L, a ferrous sulfate concentration of 0.6 mol / L, and a phosphoric acid concentration of 1.5 mol / L is obtained.

[0115] (2) Phosphoric acid is added to the mixed solution A as a chelating agent in a ratio of phosphoric acid to total iron and manganese metal ion molar amount = 1.5:1, and the mixture is stirred thoroughly. Then, ammonium persulfate is added as an oxidant in a ratio of oxidant to total iron and manganese metal ion molar amount = 1.2:1, and the mixture is stirred until the ammonium persulfate is completely dissolved. The obtained solution is filtered and allowed to stand for 12 hours to obtain a mixed solution B.

[0116] (3) Use 40% volume of mixed solution B as the base liquid, add ammonia water as the pH adjuster to the base liquid, adjust the base liquid pH to 4.0, stir it thoroughly at 350 rpm, raise the temperature to 95 °C, continue stirring and keep warm for 1.5 h to obtain a gray-green precursor slurry C.

[0117] (4) Using the gray-green precursor slurry C obtained in step (3) as the base liquid, slowly pump in the remaining 60% volume of the mixed solution B under stirring and heating conditions, and adjust the system pH to 2.0. During the reaction, the stirring speed is 350 rpm and the temperature is 85°C. After the feeding is completed, continue to keep warm for 1 hour to obtain precursor slurry D.

[0118] (5) The product obtained in step S4 is centrifuged, dried, and sieved to obtain a powder, wherein the drying temperature is 120° C. and the drying time is 12 h; the powder is calcined at 500° C. for 4 h and then naturally cooled in an air calcination atmosphere to obtain a ferromanganese phosphate material.

[0119] Figure 1 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 1. It can be seen from the figure that the characteristic peak is pure phase MnPO4·H2O.

[0120] Figure 2 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 1. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0121] Figure 3 This is a SEM image of the ferromanganese phosphate material obtained in Example 1. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical. The diameter of the primary particles of the shell is 250 nm.

[0122] Figure 4 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 1. It can be seen from the figure that the ferromanganese phosphate material is a core-shell structure, with a loose core and a dense shell, and the diameter of the primary particles of the core is significantly smaller than the diameter of the primary particles of the shell. The ratio of the thickness of the shell to the radius of the core is 1.68. The porosity of the core is further determined to be 45.8%, and the primary particles constituting the shell are dendritic.

[0123] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the amount of the complexing agent phosphoric acid added in step (2) is determined according to the molar amount of phosphoric acid: the molar amount of the total metal ions of iron and manganese = 0.8:1.

[0124] Fig.25 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 1. It can be seen from the figure that in addition to the characteristic peaks of MnPO4·H2O, there is also a (NH4)Fe2(PO4)2OH(H2O)H2O phase.

[0125] Fig.26 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 1. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0126] Fig. 27 This is a SEM image of the ferromanganese phosphate material obtained in Comparative Example 1. It can be seen from the image that the ferromanganese phosphate material has a flaky agglomerate morphology and also has a pyramidal morphology of basic iron phosphate.

[0127] Fig.28 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 1. It can be seen from the image that the ferromanganese phosphate material has no obvious core-shell structure.

[0128] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that in step (2), the amount of the oxidant ammonium persulfate added is determined according to the molar amount of ammonium persulfate: the total molar amount of manganese and iron = 0.8:1.

[0129] Fig.29 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 2. It can be seen from the figure that in addition to the characteristic peaks of MnPO4·H2O, there is also a characteristic peak of Mn(H2PO4)2.

[0130] Fig.30 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 2. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0131] Fig.31 This is a SEM image of the ferromanganese phosphate material obtained in Comparative Example 2. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical, but there are many disordered blocks on the surface.

[0132] Fig.32 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 2. It can be seen from the image that the ferromanganese phosphate material is a core-shell structure, with a loose core and a dense shell. Further determination shows that the porosity of the core is about 26.1%.

[0133] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that in step (2), the amount of the oxidant ammonium persulfate added is determined according to the molar amount of ammonium persulfate: the total molar amount of manganese and iron = 2:1.

[0134] Fig.33 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 3. It can be seen from the figure that the characteristic peak of the product is pure phase MnPO4·H2O.

[0135] Fig.34 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 3. It can be seen that the Mn, Fe, and P elements are evenly distributed.

[0136] Fig.35 This is a SEM image of the ferromanganese phosphate material obtained in Comparative Example 3. It can be seen from the image that the ferromanganese phosphate material has a block-like agglomerate morphology.

[0137] Fig.36 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 3. It can be seen from the image that the ferromanganese phosphate material basically does not have the core-shell structure.

[0138] Comparative Example 4 The only difference between Comparative Example 4 and Example 1 is that the pH value of the base liquid in step (3) is 5.5.

[0139] Fig.37 This is the XRD diagram of the ferromanganese phosphate material obtained in Comparative Example 4. It can be seen from the figure that in addition to the characteristic peaks of MnPO4·H2O, the product also has the characteristic peaks of NH4MnPO4·H2O.

[0140] Fig.38 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Comparative Example 4. It can be seen that the Mn, Fe, and P elements are evenly distributed, and there is a certain amount of N element, which is consistent with the XRD result.

[0141] Fig.39 This is a SEM image of the ferromanganese phosphate material obtained in Comparative Example 4. It can be seen from the image that the ferromanganese phosphate material has obvious phase separation.

[0142] Fig.40 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 4. It can be seen from the image that the ferromanganese phosphate material has no core-shell structure and no obvious holes inside.

[0143] Comparative Example 5 The only difference between Comparative Example 5 and Example 1 is that the pH value of the base liquid in step (3) is 1.5.

[0144] Fig.41This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 5. It can be seen from the image that the ferromanganese phosphate material has a blocky morphology and is slightly phase-separated.

[0145] Comparative Example 6 The only difference between Comparative Example 6 and Example 1 is that the temperature in step (3) is 85°C.

[0146] Fig.42 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 6. It can be seen from the image that the ferromanganese phosphate material has obvious flake and point phase separation.

[0147] Comparative Example 7 The only difference between Comparative Example 7 and Example 1 is that the temperature in step (3) is 105°C.

[0148] Fig.43 This is a SEM image of the ferromanganese phosphate material obtained in Comparative Example 7. It can be seen from the image that the ferromanganese phosphate material is an amorphous flocculent agglomerate.

[0149] Comparative Example 8 The only difference between Comparative Example 8 and Example 1 is that the pH value in step (4) is 5.5.

[0150] Fig.44 This is a SEM image of the ferromanganese phosphate material obtained in Comparative Example 8. It can be seen from the image that the ferromanganese phosphate material has a flaky morphology.

[0151] Comparative Example 9 The only difference between Comparative Example 9 and Example 1 is that the pH value in step (4) is 0.5.

[0152] Fig.45 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Comparative Example 9. It can be seen from the image that the ferromanganese phosphate material is a solid sphere.

[0153] Comparative Example 10 The only difference between Comparative Example 10 and Example 1 is that the temperature in step (4) is 55°C.

[0154] Fig.46 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 10. It can be seen from the image that the ferromanganese phosphate material has spherical and flocculent phases.

[0155] Comparative Example 11 The only difference between Comparative Example 11 and Example 1 is that the temperature in step (4) is 105°C.

[0156] Fig.47 This is the SEM image of the ferromanganese phosphate material obtained in Comparative Example 11. It can be seen from the image that the ferromanganese phosphate material has flaky and spherical phases.

[0157] Example 2 (1) According to the chemical formula Mn 0.6 Fe 0.4 PO4, add manganese chloride and ferrous sulfate to a certain amount of pure water, stir until the solution is clear, add ammonium dihydrogen phosphate in an amount equal to manganese chloride and ferrous sulfate, stir thoroughly, and then add an appropriate amount of pure water to make up the volume. Finally, a mixed solution A with a manganese chloride concentration of 1.2 mol / L, a ferrous sulfate concentration of 0.8 mol / L, and an ammonium dihydrogen phosphate concentration of 2.0 mol / L is obtained.

[0158] (2) Phosphoric acid is added as a chelating agent to the mixed solution A in a ratio of the molar amount of phosphate ion to the molar amount of the total metal ions of iron and manganese = 1.2:1, and the mixture is stirred thoroughly. Then, ammonium nitrate is added as an oxidant in a ratio of the molar amount of the oxidant to the molar amount of the total metal ions of iron and manganese = 1.2:1, and the mixture is stirred until the ammonium nitrate is completely dissolved. The resulting solution is filtered and allowed to stand for 12 hours to obtain a mixed solution B.

[0159] (3) Use 30% volume of mixed solution B as the base liquid, add ammonia water as a pH adjuster to the base liquid, adjust the base liquid pH to 3.0, stir it thoroughly at a speed of 500 rpm, raise the temperature to 95 °C, continue stirring and keep warm for 1 hour to obtain a gray-green precursor slurry C.

[0160] (4) Using the gray-green precursor slurry C obtained in step (3) as the base liquid, slowly pump in the remaining 70% volume of the mixed solution B under stirring and heating conditions, and adjust the system pH to 1.5. During the reaction, the stirring speed is 500 rpm and the temperature is 80°C. After the feeding is completed, continue to keep warm for 0.5 h to obtain precursor slurry D.

[0161] (5) The product obtained in step S4 is centrifuged, dried, and sieved to obtain a powder, wherein the drying temperature is 120° C. and the drying time is 12 h; the powder is calcined and dehydrated at 500° C. for 2 h and then naturally cooled in an air calcination atmosphere to obtain a ferromanganese phosphate material.

[0162] Figure 5 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 2. It can be seen from the figure that the characteristic peak is pure phase MnPO4·H2O.

[0163] Figure 6 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 2. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0164] Figure 7This is a SEM image of the ferromanganese phosphate material obtained in Example 2. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical. The diameter of the primary particles of the shell is 195 nm.

[0165] Figure 8 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 2. It can be seen from the figure that the ferromanganese phosphate material is a core-shell structure, with a loose core and a dense shell. The ratio of the thickness of the shell to the radius of the core is 2.70. The porosity of the shell is further measured to be 0.31%, and the secondary particle size D50 is 8.41um.

[0166] Example 3 (1) According to the chemical formula Mn 0.5 Fe 0.5 PO4, add manganese sulfate and ferrous sulfate to a certain amount of pure water, stir until the solution is clear, add phosphoric acid solution in an equal molar amount to manganese sulfate and ferrous sulfate, stir thoroughly, and then add an appropriate amount of pure water to make up the volume. Finally, a mixed solution A with a manganese sulfate concentration of 0.5 mol / L, a ferrous sulfate concentration of 0.5 mol / L, and a phosphoric acid concentration of 1 mol / L is obtained.

[0167] (2) Add diammonium hydrogen phosphate as a chelating agent to the mixed solution A at a ratio of phosphate ion molar amount: total iron and manganese metal ion molar amount = 1.5:1, and stir well. Then, add ammonium persulfate as an oxidant at a ratio of oxidant molar amount: total iron and manganese metal ion molar amount = 1.2:1, and continue stirring until the ammonium persulfate is completely dissolved. Filter the resulting solution and let it stand for 12 hours to obtain a mixed solution B.

[0168] (3) Use 20% volume of mixed solution B as the base liquid, add ammonia water as the pH adjuster to the base liquid, adjust the base liquid pH to 5.0, stir it thoroughly at 800 rpm, raise the temperature to 90 °C, continue stirring and keep warm for 2 h to obtain a gray-green precursor slurry C.

[0169] (4) Using the gray-green precursor slurry C obtained in step (3) as the base liquid, slowly pump in the remaining 80% volume of the mixed solution B under stirring and heating conditions, and adjust the system pH to 3.0. During the reaction, the stirring speed is 800 rpm and the temperature is 95°C. After the feeding is completed, continue to keep warm for 2 hours to obtain precursor slurry D.

[0170] (5) The product obtained in step S4 is centrifuged, dried, and sieved to obtain a powder, wherein the drying temperature is 120° C. and the drying time is 12 h; the powder is calcined and dehydrated at 450° C. for 4 h and then naturally cooled in an air calcination atmosphere to obtain a ferromanganese phosphate material.

[0171] Fig. 9This is the XRD diagram of the ferromanganese phosphate material obtained in Example 3. It can be seen from the figure that the characteristic peak is pure phase MnPO4·H2O.

[0172] Fig.10 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 3. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0173] Fig.11 This is a SEM image of the ferromanganese phosphate material obtained in Example 3. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical. The diameter of the primary particles of the shell is 78 nm.

[0174] Fig.12 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 3. It can be seen from the figure that the ferromanganese phosphate material is a core-shell structure, with a loose core and a dense shell. The ratio of the thickness of the shell to the radius of the core is 1.42. Further determination shows that the difference in porosity between the core and the shell is about 42%, and the particle size D50 of the secondary particles is 6.41um.

[0175] Example 4 (1) According to the chemical formula Mn 0.7 Fe 0.3 PO4, add manganese nitrate and ferrous nitrate to a certain amount of pure water, stir until the solution is clear, add ammonium dihydrogen phosphate solution in an equal molar amount to manganese nitrate and ferrous nitrate, stir thoroughly, and then add an appropriate amount of pure water to make up the volume. Finally, a mixed solution A with a manganese nitrate concentration of 1.05 mol / L, a ferrous nitrate concentration of 0.45 mol / L, and a monoammonium phosphate concentration of 1.5 mol / L is obtained.

[0176] (2) Phosphoric acid is added as a chelating agent to the mixed solution A in a ratio of phosphate ion molar amount: total iron and manganese metal ion molar amount = 1.2:1, and the mixture is stirred thoroughly. Then, hydrogen peroxide is added as an oxidant in a ratio of oxidant molar amount: total iron and manganese metal ion molar amount = 1.2:1. The obtained solution is filtered and allowed to stand for 12 hours to obtain a mixed solution B.

[0177] (3) Use 20% volume of mixed solution B as the base liquid, add ammonia water as the pH adjuster to the base liquid, adjust the base liquid pH to 3.0, stir it thoroughly at a speed of 500 rpm, raise the temperature to 95 °C, continue stirring and keep warm for 1 hour to obtain a gray-green precursor slurry C.

[0178] (4) Using the gray-green precursor slurry C obtained in step (3) as the base liquid, slowly pump in the remaining 80% volume of the mixed solution B under stirring and heating conditions, and adjust the system pH to 1.5. During the reaction, the stirring speed is 500 rpm and the temperature is 80°C. After the feeding is completed, continue to keep warm for 0.5 h to obtain precursor slurry D.

[0179] (5) The product obtained in step S4 is centrifuged, dried, and sieved to obtain a powder, wherein the drying temperature is 90° C. and the drying time is 15 h; the powder is calcined at 450° C. for 4 h and then naturally cooled in an air calcination atmosphere to obtain a ferromanganese phosphate material.

[0180] Fig.13 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 4. It can be seen from the figure that the characteristic peak is pure phase MnPO4·H2O.

[0181] Fig.14 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 4. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0182] Fig.15 This is a SEM image of the ferromanganese phosphate material obtained in Example 4. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical. The diameter of the primary particles of the shell is 470 nm.

[0183] Fig.16 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 4. It can be seen from the figure that the ferromanganese phosphate material is a core-shell structure, with a loose core and a dense shell. The ratio of the thickness of the shell to the radius of the core is 1.51. Further determination of the average aspect ratio of the shell primary particles is 2.41, and the shell primary particles are long strips.

[0184] Example 5 (1) According to the chemical formula Mn 0.6 Fe 0.4 PO4, add manganese oxalate and ferrous oxalate to a certain amount of pure water, stir until the solution is clear, add phosphoric acid solution in an equal molar amount to manganese oxalate and ferrous oxalate, stir thoroughly, and then add an appropriate amount of pure water to make up the volume. Finally, a mixed solution A with a manganese oxalate concentration of 0.9 mol / L, a ferrous oxalate concentration of 0.6 mol / L, and a phosphoric acid concentration of 1.2 mol / L is obtained.

[0185] (2) Add ammonium phosphate as a chelating agent to the mixed solution A at a ratio of phosphate ion molar amount: total iron and manganese metal ion molar amount = 2:1, and stir thoroughly; then add nitric acid as an oxidant at a ratio of oxidant molar amount: total iron and manganese metal ion molar amount = 1.2:1, filter the resulting solution, and let it stand for 12 hours to obtain a mixed solution B.

[0186] (3) Use 40% volume of mixed solution B as the base liquid, add ammonia water as a pH adjuster to the base liquid, adjust the base liquid pH to 5.0, stir it at a speed of 1000 rpm, raise the temperature to 98 °C, continue stirring and keep warm for 2 h to obtain a gray-green precursor slurry C.

[0187] (4) Using the gray-green precursor slurry C obtained in step (3) as the base liquid, slowly pump in the remaining 60% volume of the mixed solution B under stirring and heating conditions, and adjust the system pH to 3.0. During the reaction, the stirring speed is 1000 rpm and the temperature is 95°C. After the feeding is completed, continue to keep warm for 2 hours to obtain precursor slurry D.

[0188] (5) The product obtained in step S4 is centrifuged, dried, and sieved to obtain a powder, wherein the drying temperature is 150° C. and the drying time is 12 h; the powder is calcined and dehydrated at 550° C. for 2 h and then naturally cooled in an air calcination atmosphere to obtain a ferromanganese phosphate material.

[0189] Fig.17 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 5. It can be seen from the figure that the characteristic peak is pure phase MnPO4·H2O.

[0190] Fig.18 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 5. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0191] Fig.19 This is a SEM image of the ferromanganese phosphate material obtained in Example 5. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical. The diameter of the primary particles of the shell is 203 nm.

[0192] Fig. 20 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 5. It can be seen from the figure that the ferromanganese phosphate material has a core-shell structure, with a loose core and a dense shell. The ratio of the thickness of the shell to the radius of the core is 1.32. Further determination shows that the porosity of the core is 38.1%, and the secondary particle size D50 is 5.36um. Example 6 (1) According to the chemical formula Mn 0.6 Fe 0.4 PO4, add manganese acetate and ferrous acetate to a certain amount of pure water, stir until the solution is clear, add phosphoric acid solution in an equal molar amount to manganese acetate and ferrous acetate, stir thoroughly, and then add an appropriate amount of pure water to make up the volume. Finally, a mixed solution A with a manganese acetate concentration of 0.6 mol / L, a ferrous acetate concentration of 0.4 mol / L, and a phosphoric acid concentration of 1.0 mol / L is obtained.

[0193] (2) Sodium pyrophosphate was added as a chelating agent to the mixed solution A at a ratio of pyrophosphate molar amount: total iron and manganese metal ion molar amount = 1.5:1, and the mixture was stirred thoroughly. Then, ammonium persulfate was added as an oxidant at a ratio of oxidant molar amount: total iron and manganese metal ion molar amount = 1.2:1, and the mixture was stirred until the ammonium persulfate was completely dissolved. The obtained solution was filtered and allowed to stand for 12 hours to obtain a mixed solution B.

[0194] (3) Use 30% volume of mixed solution B as the base liquid, add ammonia water as a pH adjuster to the base liquid, adjust the base liquid pH to 3.5, stir it thoroughly at a speed of 500 rpm, raise the temperature to 95 °C, continue stirring and keep warm for 1.5 h to obtain a gray-green precursor slurry C.

[0195] (4) Using the gray-green precursor slurry C obtained in step (3) as the base liquid, slowly pump in the remaining 70% volume of the mixed solution B under stirring and heating conditions, and adjust the system pH to 2.7. During the reaction, the stirring speed is 800 rpm and the temperature is 90°C. After the feeding is completed, continue to keep warm for 2 hours to obtain precursor slurry D.

[0196] (5) The product obtained in step S4 is centrifuged, dried, and sieved to obtain a powder, wherein the drying temperature is 100° C. and the drying time is 15 h; the powder is calcined at 480° C. for 4 h and then naturally cooled in an air calcination atmosphere to obtain a ferromanganese phosphate material.

[0197] Fig.21 This is the XRD diagram of the ferromanganese phosphate material obtained in Example 6. It can be seen from the figure that the characteristic peak is pure phase MnPO4·H2O.

[0198] Fig. 22 This is the EDS diagram of each element in the ferromanganese phosphate material obtained in Example 6. It can be seen that the Mn, Fe and P elements are evenly distributed.

[0199] Fig.23 This is a SEM image of the ferromanganese phosphate material obtained in Example 6. It can be seen from the image that the ferromanganese phosphate material is spherical or quasi-spherical. The diameter of the primary particles of the shell is 123 nm.

[0200] Fig.24 This is a cross-sectional SEM image of the ferromanganese phosphate material obtained in Example 6. It can be seen from the figure that the ferromanganese phosphate material is a core-shell structure, with a loose core and a dense shell. The ratio of the thickness of the shell to the radius of the core is 0.84. Further determination shows that the difference in porosity between the core and the shell is 42%, and the primary particles of the shell are strip-shaped.

[0201] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing ferromanganese phosphate, characterized in that: include: Step S1, adding a complexing agent and an oxidant to a mixed solution A of a manganese source, an iron source, and a phosphorus source to obtain a mixed solution B; Step S2, dividing the mixed solution B into two parts, a mixed solution B-1 and a mixed solution B-2; Step S3, adjusting the pH value of the mixed solution B-1 to 2.0-5.0, heating to 90-100° C., and keeping the temperature to obtain slurry I; Step S4, adding the mixed solution B-2 to the slurry I, adjusting the pH value of the system to 1-5, and keeping the temperature at 60-100° C. to obtain slurry II; Step S5, separating the slurry II into solid and liquid, drying, screening and calcining the obtained solid phase to obtain ferromanganese phosphate.

2. The method for preparing ferromanganese phosphate according to claim 1, characterized in that: The total molar concentration of manganese and iron in the mixed solution A is 0.2-2.0 mol / L; Preferably, the molar ratio of manganese to iron in the mixed solution A is 1-2:

1.

3. The method for preparing ferromanganese phosphate according to claim 1 or 2, characterized in that: The ratio of the molar amount of the complexing agent to the total molar amount of iron and manganese is 1-2:1; Preferably, the ratio of the molar amount of the oxidant to the total molar amount of iron and manganese is 1-1.5:

1.

4. The method for preparing ferromanganese phosphate according to any one of claims 1 to 3, characterized in that: The volume ratio of the mixed solution B-1 to the mixed solution B-2 is (20~40):(80~60); Preferably, in step S3, the pH value of the mixed solution B-1 is adjusted to 3.0-5.0; Preferably, in step S3, heating is performed to 95-100° C.; Preferably, in step S3, the holding time is 1 to 2 hours; Preferably, in step S4, the pH value of the system is adjusted to 1.5-3.

0. Preferably, in step S4, the temperature is kept at 80-95°C; Preferably, in step S4, the holding time is 0.5 to 2 hours; Preferably, stirring is performed during step S1, step S3 and step S4; preferably, the stirring speed is 100-1000 rpm.

5. The method for preparing ferromanganese phosphate according to any one of claims 1 to 4, characterized in that: In step S5, the drying temperature is 90-150°C; Preferably, the calcination temperature is 200-600°C.

6. A ferromanganese phosphate, characterized in that: The chemical formula of the ferromanganese phosphate is Mn x Fe 1-x PO4, wherein 0.1≤x≤0.9, preferably 0.4≤x≤0.8; the manganese iron phosphate is a secondary particle formed by agglomeration of primary particles, and has a spherical or quasi-spherical structure; it includes an inner core and an outer shell, the inner core is loose and porous, and the outer shell is relatively compact.

7. The ferromanganese phosphate according to claim 6, characterized in that The diameter of the primary particle of the shell is 100-500 nm; the diameter of the primary particle of the core is smaller than the diameter of the primary particle of the shell; Preferably, the ratio of the thickness of the outer shell to the radius of the inner core is 0.8-3.0:

1.

8. Ferromanganese phosphate according to claim 6 or 7, characterized in that The ferromanganese phosphate satisfies at least one of the following conditions (a) to (c): (a) the porosity of the inner core is 30-60%, preferably 40-50%; (b) The porosity of the shell is 0.01-5%, preferably 0.05-2%; (c) The porosity difference between the core and the shell is 25-60%, preferably 40-50%; And / or, the ferromanganese phosphate satisfies at least one of the following conditions (d) to (f): (d) the primary particles constituting the shell are in the shape of dendrites or strips; (e) the average aspect ratio of the primary particles constituting the shell is 1.0 to 4.0, preferably 1.5 to 3.0; (f) The particle size D50 of the secondary particles is 5.0-9.0 μm.

9. A positive electrode material, characterized in that: The ferromanganese phosphate is prepared by the preparation method according to any one of claims 1 to 5 or the ferromanganese phosphate according to any one of claims 6 to 8.

10. A battery, characterized in that: Comprising the positive electrode material according to claim 9.

Citation Information

Patent Citations

  • Radial nickel-based precursor and preparation method thereof

    CN113823779A

  • Preparation method of lithium manganese iron phosphate positive electrode material

    CN114380280A

  • Lithium manganese iron phosphate positive electrode material as well as positive plate and battery comprising same

    CN114530595A

  • Battery positive electrode material as well as preparation method and application thereof

    CN115911291A

  • Ferromanganese phosphate as well as preparation method, production system device and application thereof

    CN116281925A

Cited By

  • Preparation method of sodium ferromanganese phosphate-pyrophosphate positive electrode material

    CN119569014A

  • Method for preparing ferromanganese phosphate from waste ferrophosphorus slag

    CN120646801A

  • Method for preparing manganese iron phosphate by using waste phosphorus iron slag

    CN120646801B

  • Ferromanganese phosphate precursor as well as preparation method and application thereof