Highly waterproof environment-friendly packaging carton and preparation method thereof

By spraying modified water-based polyurethane emulsion and other materials on the packaging paper box, a high waterproof and environmentally friendly packaging paper box is solved, and the problem of difficulty in meeting waterproof and environmental protection in the existing technology is solved, and the efficient waterproof and antibacterial materials are achieved. and flame retardant properties meet the needs of the food packaging industry while reducing production costs.

CN118932787AActive Publication Date: 2024-11-12龙海市新德纸品有限公司

Patent Information

Application Number
CN202411020170.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

Existing packaging paper boxes are difficult to meet the requirements of high waterproofing and environmental protection at the same time, especially in humid areas, and there are flammable and food safety hazards.

Method used

Waterproof and antibacterial coating composed of modified water-based polyurethane emulsion, carboxymethyl chitosan, modified polylactic acid, composite antibacterial agent and silane coupling agent is sprayed on the surface of the cardboard layer and cured to form a highly waterproof and environmentally friendly packaging paper box. Material.

Benefits of technology

It achieves excellent hydrophobic properties, antibacterial properties, flame retardancy and environmental protection of the material, meets the high standard needs of the food packaging industry, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the field of packaging cartons, in particular to a high-waterproof environment-friendly packaging carton material and a preparation method thereof. A highly waterproof environment-friendly packaging carton material comprises a paperboard layer and a waterproof antibacterial layer coated on the surface of the paperboard layer, the thickness of the waterproof antibacterial layer is 30-50 microns, the waterproof antibacterial layer is prepared by spraying waterproof antibacterial coating on the surface of the paperboard layer and curing the waterproof antibacterial coating, and the waterproof antibacterial coating comprises the following components in parts by mass: 1-5 parts of a waterproof antibacterial agent, 1-5 parts of a curing agent and 1-5 parts of a curing agent. Comprising the following preparation raw materials: 100-110 parts of a modified waterborne polyurethane emulsion, 3-5 parts of carboxymethyl chitosan, 8-10 parts of modified polylactic acid, 1-2 parts of a composite antibacterial agent and 0.5-0.8 part of a silane coupling agent, and the composite antibacterial agent is composed of modified silver and cerium doped titanium dioxide and peppermint oil. The highly-waterproof environment-friendly packaging carton material integrates multiple functions, such as water resistance, bacteria resistance, flame retardance, environmental protection and safety, has good mechanical performance and durability, is very suitable for the requirements of the food packaging industry, and has wide market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of packaging paper boxes, and in particular to a highly waterproof and environmentally friendly packaging paper box material and a preparation method thereof. Background Art

[0002] As an important part of logistics and commodity circulation, the performance of packaging cartons is crucial to the protection of products and the impact on the environment. With the improvement of environmental awareness, the market has put forward higher requirements on the environmental performance of packaging cartons. At the same time, in humid or rainy areas, the waterproof performance of packaging cartons is also particularly important. However, packaging cartons in the prior art often find it difficult to meet the requirements of high waterproofness and environmental protection at the same time.

[0003] For example, paper packaging boxes used in the catering industry need to have good waterproof, oil-proof and antibacterial properties; and existing paper packaging boxes usually add fluorine-containing oil-proof agents and water-repellent agents to improve the waterproof and oil-resistant properties of the packaging boxes, but they contain trace amounts of perfluorooctanoic acid and perfluorooctane sulfonate, which pose a risk of being transferred to the human body with food, which is not conducive to food safety and human health; and paper packaging boxes also have the problem of being easy to burn. How to improve the waterproof, oil-proof, antibacterial and flame retardant properties of paper packaging boxes is also a research hotspot in this field. Summary of the invention

[0004] The purpose of this application is to provide a highly waterproof and environmentally friendly packaging paper box material and a preparation method thereof in response to the deficiencies of current technology. The preparation method of the highly waterproof and environmentally friendly packaging paper box material of the present application has the advantages of simple production and low cost. At the same time, the highly waterproof and environmentally friendly packaging paper box material has excellent hydrophobic properties, antibacterial properties, flame retardancy and environmental safety, meeting the needs of the food packaging industry.

[0005] In the first aspect, the present application provides a highly waterproof and environmentally friendly packaging paper box material, which adopts the following technical solution: A highly waterproof and environment-friendly packaging paper box material comprises a paperboard layer and a waterproof and antibacterial layer coated on the surface of the paperboard layer, wherein the thickness of the waterproof and antibacterial layer is 30-50 microns, and the waterproof and antibacterial layer is prepared by spraying a waterproof and antibacterial coating on the surface of the paperboard layer and curing the coating, wherein the waterproof and antibacterial coating comprises the following raw materials by weight: 100-110 parts of a modified waterborne polyurethane emulsion, 3-5 parts of carboxymethyl chitosan, 8-10 parts of a modified polylactic acid, 1-2 parts of a composite antibacterial agent, and 0.5-0.8 parts of a silane coupling agent, wherein the composite antibacterial agent consists of modified silver cerium doped titanium dioxide and peppermint oil.

[0006] By adopting the above technical scheme, modified waterborne polyurethane emulsion: as the main component of waterproof and antibacterial coating, modified waterborne polyurethane emulsion introduces di-terminal hydroxybutyl polydimethylsilane through mini-emulsion polymerization, which improves the compatibility between polyurethane chains and polyacrylate chains and reduces the degree of phase separation. This modification not only improves the waterproofness, oil resistance and flexibility of the material, but also gives the packaging carton material a higher self-healing property. Carboxymethyl chitosan: effectively improves the antibacterial and oil repellency of packaging carton materials. Carboxymethyl chitosan is a natural polymer compound with good biocompatibility and biodegradability, which makes it have important applications in environmentally friendly materials. Modified polylactic acid: polylactic acid is an environmentally friendly polymer material, but it is relatively brittle and has poor aging resistance. In this application, composite phytates are synthesized by citrulline, phytic acid, and genipin, and polylactic acid is modified together with tannic acid to improve its toughening effect. The addition of tannic acid and composite phytate effectively improves the flame retardancy of the waterproof and antibacterial layer, and the tannic acid introduced in the modified polylactic acid undergoes a free radical grafting reaction with the sodium alginate in the carboxymethyl chitosan, which enhances the complexity of the network construction of the waterproof and antibacterial layer, improves the performance uniformity of the waterproof and antibacterial coating, and improves the bonding strength with the cardboard layer, extending the service life. Composite antibacterial agent (modified silver cerium doped titanium dioxide and peppermint oil): modified silver cerium doped titanium dioxide has excellent antibacterial properties, photocatalytic properties and dispersibility, and has good compatibility with other components of the waterproof and antibacterial coating. Peppermint oil, as a natural antibacterial agent, works together with modified silver cerium doped titanium dioxide to provide a good antibacterial effect. Silane coupling agent: As a cross-linking agent, it improves the interaction between different components, enhances the bonding strength between the coating and the cardboard layer, and ensures the stability and durability of the coating. In summary, the highly waterproof and environmentally friendly packaging paper box material of the present application not only achieves excellent hydrophobicity, antibacterial properties and flame retardancy through the synergistic effect of various components, but also takes into account environmental protection and safety, meeting the high standards of the food packaging industry.

[0007] Preferably, the mass ratio of the modified silver-cerium doped titanium dioxide to the peppermint oil is 3:2.

[0008] By adopting the above technical scheme, the modified silver-cerium doped titanium dioxide has excellent antibacterial properties. Silver ions and cerium ions are both known powerful antibacterial agents, which can inhibit the growth and reproduction of bacteria by destroying the cell wall and cell membrane of bacteria. Titanium dioxide is a commonly used photocatalyst that can produce free radicals under ultraviolet light irradiation, which can decompose organic matter, thereby achieving antibacterial and self-cleaning functions. The doping of silver and cerium further improves the photocatalytic activity of titanium dioxide, allowing it to work in the visible light range. The modified silver-cerium doped titanium dioxide has good dispersibility, which helps to be evenly distributed in the waterproof antibacterial coating to ensure that the entire coating has consistent antibacterial properties. Peppermint oil contains a variety of compounds with antibacterial activity, such as menthol, which can effectively inhibit or kill microorganisms. Peppermint oil has a fresh aroma, which can add a certain fragrance to packaging materials and enhance user experience. Modified silver-cerium doped titanium dioxide mainly targets bacteria, while the natural antibacterial ingredients in peppermint oil can act on a variety of microorganisms including bacteria and fungi. The combination of the two can broaden the antibacterial spectrum and improve the antibacterial effect. The compounds in peppermint oil can destroy the cell membrane of microorganisms and increase the permeability of the cell membrane, making it easier for silver ions and cerium ions to enter the interior of bacterial cells and enhance the antibacterial effect. The photocatalytic properties of modified silver-cerium doped titanium dioxide combined with the chemical antibacterial effect of peppermint oil can provide continuous antibacterial protection under different environmental conditions. In summary, the combination of modified silver-cerium doped titanium dioxide and peppermint oil in a mass ratio of 3:2 can not only provide broad-spectrum and efficient antibacterial protection, but also utilize their respective characteristics to enhance the overall antibacterial effect through synergistic effects, while bringing additional functions and user experience to packaging materials.

[0009] Preferably, the material of the paperboard layer is one of sack paper, kraft paper, kraft cardboard, boxboard and corrugated paper.

[0010] Preferably, the thickness of the paperboard layer is 200-400 microns.

[0011] Preferably, the preparation method of the modified aqueous polyurethane emulsion comprises the following steps: S51, according to the mass parts, 71 parts of di-terminal hydroxybutyl polydimethylsilane, 114 parts of butyl acrylate, 61 parts of styrene, 89 parts of polycaprolactone, 33 parts of isophorone diisocyanate, 3 parts of hydroxyethyl methacrylate, 1.8 parts of azobisisobutyronitrile, 0.5 parts of dibutyltin dilaurate and 10.5 parts of n-hexadecane were mixed uniformly to obtain a mixture; S52. Add the mixture into 300 parts of an aqueous emulsifier solution with a mass concentration of 6%, and then pre-emulsify at 3000r / min to obtain a crude emulsion, and then use a cell crusher to ultrasonically treat it in an ice-water bath for 40 minutes to obtain a monomer fine emulsion. Finally, stir the obtained monomer fine emulsion in a nitrogen atmosphere for 1.5 hours, transfer it to a three-necked flask, maintain the temperature at 72°C, and carry out a fine emulsion polymerization reaction in a nitrogen environment for 10 hours to obtain a modified waterborne polyurethane emulsion.

[0012] By adopting the above technical scheme, the preparation method of the present application successfully introduces di-terminal hydroxybutyl polydimethylsilane into the polyurethane segment through mini-emulsion polymerization to obtain a modified aqueous polyurethane emulsion. This method not only improves the compatibility between the polyurethane chain and the polyacrylate chain, but also reduces the degree of phase separation, thereby enhancing the waterproof, oil-proof and flexibility of the waterproof and antibacterial layer. At the same time, by introducing hydrophobic di-terminal hydroxybutyl polydimethylsilane, it can also effectively inhibit water molecules and oil molecules from penetrating from the surface of the highly waterproof and environmentally friendly packaging paper box material to the inside, further improving its waterproof performance.

[0013] Preferably, the emulsifier is 1-allyloxy-3-4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate.

[0014] Preferably, the preparation method of the modified silver-cerium doped titanium dioxide comprises the following steps: S71. At room temperature, add 100 mL of tetra-n-butyl titanate to a solution consisting of 160 mL of ethanol and 30 mL of deionized water, and stir for 30 min to form solution A. S72, adding 1.5 g of silver nitrate and 12 g of cerium nitrate to a solution consisting of 100 mL of ethanol, 15 mL of acetic acid and 45 mL of water to form solution B; S73, adding solution B dropwise into solution A, stirring for 60 min, heating to 42° C., standing for 12 h, then centrifuging, washing, and drying at 80° C. for 12 h to obtain silver-cerium-doped titanium dioxide; S74, mixing 0.8 g of γ-(methacryloyloxy)propyltrimethoxysilane with 70 g of ethanol and 8 g of water, and hydrolyzing for 4 h to obtain a mixture C; S75. Add the obtained silver-cerium-doped titanium dioxide to mixture C, then heat it to 43°C, stir it at 300 r / min for 250 min, and finally filter, wash, dry and grind it at 85°C to obtain modified silver-cerium-doped titanium dioxide with an average particle size of 40 nanometers.

[0015] By adopting the above technical scheme, the modified silver-cerium doped titanium dioxide has excellent antibacterial properties. Silver ions and cerium ions are both known powerful antibacterial agents, which can inhibit the growth and reproduction of bacteria by destroying the cell walls and cell membranes of bacteria. Titanium dioxide is a commonly used photocatalyst that can produce free radicals under ultraviolet light irradiation. These free radicals can decompose organic matter and achieve antibacterial and self-cleaning functions. The doping of silver and cerium further improves the photocatalytic activity of titanium dioxide, allowing it to work in the visible light range. The modified silver-cerium doped titanium dioxide has good dispersibility, which helps to be evenly distributed in the waterproof and antibacterial coating to ensure that the entire coating has consistent antibacterial properties. The modified silver-cerium doped titanium dioxide has good compatibility with other components in the waterproof and antibacterial coating, and can synergize with other ingredients such as modified water-based polyurethane emulsions, carboxymethyl chitosan, etc. to jointly improve the waterproof, antibacterial and flame retardant properties of the coating. In summary, modified silver-cerium doped titanium dioxide plays a key role in highly waterproof and environmentally friendly packaging carton materials through its antibacterial properties, photocatalytic properties and good dispersibility, and synergizes with other components to jointly improve the overall performance of the material.

[0016] Preferably, the silane coupling agent is composed of isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane in a mass ratio of 3:4.

[0017] By adopting the above technical scheme, the main function of the silane coupling agent is to act as a cross-linking agent to improve the adhesion between different materials. In this material, it effectively improves the bonding force between the waterproof and antibacterial coating and the paperboard layer, ensuring that the coating is firmly attached to the paperboard and is not easy to peel off. Isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane are both hydrophobic compounds that can reduce the permeability of water molecules to the coating, thereby enhancing the water resistance of the overall material. By promoting the formation of chemical bonds between the coating and the paperboard, the silane coupling agent helps to enhance the mechanical strength of the coating, such as wear resistance and impact resistance. The silane coupling agent can also improve the aging resistance of the material and extend the service life of the packaging carton. Isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane each have different functional groups. The oleic acid acyl group of the former and the methacryloyl group of the latter can react with different material surfaces to form strong chemical bonds. Isopropyl trioleyl titanate has strong hydrophobicity, while γ-(methacryloyloxy)propyl trimethoxy silane has certain hydrophilicity. This combination helps to form a balanced interface between the coating and the paperboard, which can effectively repel moisture and ensure good adhesion between the coating and the paperboard. Both have good chemical stability and can maintain their chemical structure unchanged under various environments, thus ensuring the stability and durability of the coating. By adjusting the ratio of the two silane coupling agents, the compatibility of the interface between the coating and the paperboard can be optimized to achieve the best bonding effect. In summary, the use of silane coupling agents not only improves the overall performance of the material, but also optimizes the combination of the coating and the paperboard through the synergistic effect between its components, enhances the water resistance, mechanical properties and aging resistance of the material, while maintaining environmental protection characteristics, meeting the needs of the food packaging industry.

[0018] Preferably, the preparation method of the modified polylactic acid comprises the following steps: S91, according to the mass parts, 131 parts of phytic acid solution with a mass concentration of 70%, 4.6 parts of citrulline, and 0.3 parts of genipin were mixed, the temperature was raised to 88°C and kept warm for 5 hours, purified with ethanol, filtered, and dried to obtain a phytic acid composite salt; S92. According to the weight ratio, 10 parts of tannic acid and 90 parts of phytic acid composite salt are mixed, and 900 parts of polylactic acid are added, and the mixture is mixed in a high-speed mixer to obtain modified polylactic acid.

[0019] By adopting the above technical scheme, the toughness of the material can be effectively improved by adding a modifier composed of tannic acid and phytic acid composite salt to polylactic acid. This is because tannic acid and phytic acid composite salt can act as plasticizers to increase the mobility between polymer chains, thereby reducing the brittleness of the material. Tannic acid and phytic acid composite salt can act as flame retardants in the material. In particular, tannic acid, which is a natural flame retardant, can improve the thermal stability and flame retardancy of the material. The phytic acid composite salt in the modified polylactic acid has good water resistance, which helps to improve the waterproof performance of the overall material. The tannic acid in the modified polylactic acid undergoes a free radical grafting reaction with the sodium alginate in the carboxymethyl chitosan. This chemical reaction enhances the interaction between different layers and improves the adhesion between the layers. The grafting reaction increases the complexity of the internal structure of the material and forms a more stable network structure, which not only improves the overall performance of the material, but also helps to evenly disperse the applied pressure or impact. Due to the characteristics of the above-mentioned modified polylactic acid, it can effectively extend the service life of the packaging carton, especially in terms of resistance to environmental factors (such as water, fire) and wear during use. In summary, the introduction of modified polylactic acid not only improves the physical and chemical properties of packaging cartons, but also optimizes the overall function of the material through synergistic effects with other ingredients, making it more suitable for the needs of the food packaging industry.

[0020] In a second aspect, the present application provides a method for preparing a highly waterproof and environmentally friendly packaging paper box material, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned highly waterproof and environmentally friendly packaging paper box material, comprising the following steps: S101, uniformly stirring the modified waterborne polyurethane emulsion, carboxymethyl chitosan, modified polylactic acid, composite antibacterial agent and silane coupling agent according to their weight proportions to obtain a waterproof and antibacterial coating; S102, spraying the waterproof and antibacterial coating on the surface of the paperboard layer, and then drying it at 80-85° C. for 60-70 minutes to form a waterproof layer through a drying and curing process to obtain a highly waterproof and environmentally friendly packaging paper box material.

[0021] In summary, the beneficial technical effects of this application are: 1. Excellent hydrophobic properties: Through the preparation and application of modified waterborne polyurethane emulsion, the introduction of di-terminal hydroxybutyl polydimethylsilane significantly improves the hydrophobic properties of the material. This hydrophobic material can effectively prevent the penetration of moisture and oil, thereby protecting the contents of the package from contamination, and is particularly suitable for food packaging that requires moisture or oil resistance.

[0022] 2. Excellent antibacterial and photocatalytic properties: The addition of carboxymethyl chitosan, modified silver cerium doped titanium dioxide and peppermint oil improves the antibacterial properties of the material. These antimicrobial agents have the ability to destroy bacterial cell walls, thereby inhibiting the growth of microorganisms, which is essential to ensure the hygienic safety of food packaging. The photocatalytic properties of modified silver cerium doped titanium dioxide can be used to decompose organic matter, achieve self-cleaning function, reduce maintenance costs and extend service life.

[0023] 3. Improved flame retardancy: The combined effect of tannic acid and complex phytates enhances the flame retardancy of the material. In the event of a fire, the material can burn more slowly, providing more time for rescue and reducing the risk of fire.

[0024] 4. Improved durability: The introduction of modified polylactic acid solves the problems of polylactic acid's high brittleness and poor aging resistance, and increases the material's flexibility and service life. This means that the packaging material can better withstand pressure and impact during use and is not easily damaged.

[0025] 5. Environmentally friendly: The materials used, such as polylactic acid, are biodegradable, which is in line with the current environmental protection trend. This helps reduce the impact of plastic waste on the environment and is in line with the goal of sustainable development.

[0026] 6. Cost-effectiveness: The preparation method is simple and the cost is low, making this material suitable for large-scale production. This not only reduces the production cost, but also makes the environmentally friendly material more easily accepted by the market.

[0027] 7. Self-repairability: The material has a high degree of self-repairability and can self-repair small damages to a certain extent, which further enhances its durability and practicality. DETAILED DESCRIPTION

[0028] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0029] Preparation Example 1 Preparation of modified waterborne polyurethane emulsion The preparation method of the modified waterborne polyurethane emulsion comprises the following steps: S51, according to the mass parts, 71g of di-terminal hydroxybutyl polydimethylsilane, 114g of butyl acrylate, 61g of styrene, 89g of polycaprolactone, 33g of isophorone diisocyanate, 3g of hydroxyethyl methacrylate, 1.8g of azobisisobutyronitrile, 0.5g of dibutyltin dilaurate and 10.5g of n-hexadecane were mixed uniformly to obtain a mixture; S52. Add the mixture into 300 g of 6% 1-allyloxy-3-4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate aqueous solution, then pre-emulsify at 3000 r / min to obtain a crude emulsion, and then use a cell crusher to ultrasonically treat it in an ice water bath for 40 minutes to obtain a monomer fine emulsion. Finally, stir the obtained monomer fine emulsion in a nitrogen atmosphere for 1.5 hours, transfer it to a three-necked flask, maintain the temperature at 72°C and carry out a fine emulsion polymerization reaction in a nitrogen environment for 10 hours to obtain a modified waterborne polyurethane emulsion.

[0030] Preparation Example 2 Preparation of modified silver-cerium doped titanium dioxide The preparation method of modified silver-cerium doped titanium dioxide comprises the following steps: S71. At room temperature, add 100 mL of tetra-n-butyl titanate to a solution consisting of 160 mL of ethanol and 30 mL of deionized water, and stir for 30 min to form solution A. S72, adding 1.5 g of silver nitrate and 12 g of cerium nitrate to a solution consisting of 100 mL of ethanol, 15 mL of acetic acid and 45 mL of water to form solution B; S73, adding solution B dropwise into solution A, stirring for 60 min, heating to 42° C., standing for 12 h, then centrifuging, washing, and drying at 80° C. for 12 h to obtain silver-cerium-doped titanium dioxide; S74, mixing 0.8 g of γ-(methacryloyloxy)propyltrimethoxysilane with 70 g of ethanol and 8 g of water, and hydrolyzing for 4 h to obtain a mixture C; S75. Add the obtained silver-cerium-doped titanium dioxide to mixture C, then heat it to 43°C, stir it at 300 r / min for 250 min, and finally filter, wash, dry and grind it at 85°C to obtain modified silver-cerium-doped titanium dioxide with an average particle size of 40 nanometers.

[0031] Preparation Example 3 Preparation of modified polylactic acid The preparation method of modified polylactic acid comprises the following steps: S91, according to the mass fractions, 131g of phytic acid solution with a mass concentration of 70%, 4.6g of citrulline, and 0.3g of genipin were mixed, the temperature was raised to 88°C and kept warm for 5h, purified with ethanol, filtered, and dried to obtain a phytic acid composite salt; S92. According to the mass fractions, 10 g of tannic acid and 90 g of phytic acid composite salt were mixed, and 900 g of polylactic acid was added, and the mixture was mixed in a high-speed mixer to obtain modified polylactic acid.

[0032] Preparation Example Comparative Example 1 Preparation of Aqueous Polyurethane Emulsion The preparation method of waterborne polyurethane emulsion comprises the following steps: S51, according to the mass parts, 114g butyl acrylate, 61g styrene, 89g polycaprolactone, 33g isophorone diisocyanate, 3g hydroxyethyl methacrylate, 1.8g azobisisobutyronitrile, 0.5g dibutyltin dilaurate and 10.5g n-hexadecane were mixed uniformly to obtain a mixture; S52. Add the mixture into 300 g of 6% 1-allyloxy-3-4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate aqueous solution, then pre-emulsify at 3000 r / min to obtain a crude emulsion, and then use a cell crusher to ultrasonically treat it in an ice water bath for 40 minutes to obtain a monomer fine emulsion. Finally, stir the obtained monomer fine emulsion in a nitrogen atmosphere for 1.5 hours, transfer it to a three-necked flask, maintain the temperature at 72°C and carry out a fine emulsion polymerization reaction in a nitrogen environment for 10 hours to obtain a modified waterborne polyurethane emulsion.

[0033] Example 1 A highly waterproof and environment-friendly packaging paper box material comprises a paperboard layer and a waterproof and antibacterial layer coated on the surface of the paperboard layer, wherein the waterproof and antibacterial layer has a thickness of 30 microns and is prepared by spraying a waterproof and antibacterial coating on the surface of the paperboard layer and curing the coating, wherein the waterproof and antibacterial coating comprises the following raw materials by mass: 100 g of a modified aqueous polyurethane emulsion, 3 g of carboxymethyl chitosan, 8 g of modified polylactic acid, 1 g of a composite antibacterial agent, and 0.5 g of a silane coupling agent, wherein the composite antibacterial agent is composed of modified silver cerium-doped titanium dioxide and peppermint oil in a mass ratio of 3:2, the paperboard layer is a paper bag paper with a thickness of 400 microns, and the silane coupling agent is composed of isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane in a mass ratio of 3:4.

[0034] The method for preparing the above-mentioned highly waterproof and environmentally friendly packaging paper box material comprises the following steps: S101, uniformly stirring the modified waterborne polyurethane emulsion, carboxymethyl chitosan, modified polylactic acid, composite antibacterial agent and silane coupling agent according to their weight proportions to obtain a waterproof and antibacterial coating; S102, spraying the waterproof and antibacterial coating on the surface of the paperboard layer, and then drying it at 80° C. for 70 minutes to form a waterproof layer through a drying and curing process to obtain a highly waterproof and environmentally friendly packaging paper box material.

[0035] Example 2 A highly waterproof and environment-friendly packaging paper box material comprises a paperboard layer and a waterproof and antibacterial layer coated on the surface of the paperboard layer, wherein the waterproof and antibacterial layer has a thickness of 50 microns and is prepared by spraying a waterproof and antibacterial coating on the surface of the paperboard layer and curing the coating, wherein the waterproof and antibacterial coating comprises the following raw materials by mass: 110 g of a modified aqueous polyurethane emulsion, 5 g of carboxymethyl chitosan, 10 g of a modified polylactic acid, 2 g of a composite antibacterial agent, and 0.8 g of a silane coupling agent, wherein the composite antibacterial agent is composed of modified silver cerium-doped titanium dioxide and peppermint oil in a mass ratio of 3:2, the paperboard layer is kraft paper with a thickness of 200 microns, and the silane coupling agent is composed of isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane in a mass ratio of 3:4.

[0036] The method for preparing the above-mentioned highly waterproof and environmentally friendly packaging paper box material comprises the following steps: S101, uniformly stirring the modified waterborne polyurethane emulsion, carboxymethyl chitosan, modified polylactic acid, composite antibacterial agent and silane coupling agent according to their weight proportions to obtain a waterproof and antibacterial coating; S102, spraying the waterproof and antibacterial coating on the surface of the paperboard layer, and then drying it at 85° C. for 60 minutes to form a waterproof layer through a drying and curing process to obtain a highly waterproof and environmentally friendly packaging paper box material.

[0037] Example 3 A highly waterproof and environment-friendly packaging paper box material comprises a paperboard layer and a waterproof and antibacterial layer coated on the surface of the paperboard layer, wherein the waterproof and antibacterial layer has a thickness of 40 microns and is prepared by spraying a waterproof and antibacterial coating on the surface of the paperboard layer and curing the coating, wherein the waterproof and antibacterial coating comprises the following raw materials by mass: 105 g of a modified aqueous polyurethane emulsion, 4 g of carboxymethyl chitosan, 9 g of modified polylactic acid, 1.5 g of a composite antibacterial agent, and 0.6 g of a silane coupling agent, wherein the composite antibacterial agent is composed of modified silver cerium-doped titanium dioxide and peppermint oil in a mass ratio of 3:2, the paperboard layer is a boxboard paper with a thickness of 300 microns, and the silane coupling agent is composed of isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane in a mass ratio of 3:4.

[0038] The method for preparing the above-mentioned highly waterproof and environmentally friendly packaging paper box material comprises the following steps: S101, uniformly stirring the modified waterborne polyurethane emulsion, carboxymethyl chitosan, modified polylactic acid, composite antibacterial agent and silane coupling agent according to their weight proportions to obtain a waterproof and antibacterial coating; S102, spraying the waterproof and antibacterial coating on the surface of the paperboard layer, and then drying it at 83° C. for 65 minutes to form a waterproof layer through a drying and curing process to obtain a highly waterproof and environmentally friendly packaging paper box material.

[0039] Comparative Example 1 The same as Example 3, except that the composite antibacterial agent is modified silver-cerium doped titanium dioxide.

[0040] Comparative Example 2 The same as Example 3, except that the composite antibacterial agent is peppermint oil.

[0041] Comparative Example 3 The same as Example 3, except that the silane coupling agent is isopropyl trioleate titanate.

[0042] Comparative Example 4 The same as Example 3, except that the silane coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane.

[0043] Comparative Example 5 The same as Example 3, except that an equal amount of the aqueous polyurethane emulsion prepared in Preparation Example Comparative Example 1 is used instead of the modified aqueous polyurethane emulsion.

[0044] Comparative Example 6 The same as Example 3, except that an equal amount of polylactic acid is used instead of modified polylactic acid.

[0045] Performance Testing The highly waterproof and environment-friendly packaging paper box materials prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were sampled and subjected to the following tests. The test results are shown in Table 1.

[0046] Flame retardancy test: Cut the sample to be tested into 100×8×2mm 3 , put it into a glass combustion tube, pass a nitrogen and oxygen mixed flow, record the minimum oxygen concentration required for combustion, and take the average value of five tests for each group; Hydrophobicity test: 3 μL of deionized water was used as the solvent, and the contact angle was measured with a residence time of 3 s. The result was the average value of five different positions on the surface. The detection method of the antibacterial rate refers to the oscillation method in the GB / T20944.3-2008 standard for antibacterial experiments; Self-healing test: scratch the surface of the protective layer with a length of 400 μm and a depth of 20 μm, keep it in a 50°C oven for 12 hours, observe with an optical microscope and record the repair rate; Hot water permeability test: refer to GB / T36787-2018, place the sample to be tested on a flat plate lined with filter paper, pour 100℃ hot water into it, let it stand for 30 minutes, observe whether there is deformation, whether there is seepage or leakage on the back, if there is no, it is considered qualified, take 10 samples from each group, and record the qualified rate; Hot oil permeability test: refer to GB / T36787-2018, place the sample to be tested on a flat plate lined with filter paper, pour in 100℃ hot oil, let it stand for 30 minutes, observe whether there is any deformation and whether there is oil print on the back, take 10 samples in each group and record the qualified rate.

[0047] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The highly waterproof and environment-friendly packaging paper box materials prepared in Examples 1 to 3 have excellent hydrophobic properties, antibacterial properties, flame retardancy and environmental safety, meeting the needs of the food packaging industry.

[0048] 2) The performance comparison analysis of the highly waterproof and environmentally friendly packaging paper box materials prepared in combination with Example 3 and Comparative Examples 1-2 shows that the modified silver cerium-doped titanium dioxide and peppermint oil are used in a mass ratio of 3:2. By utilizing the synergistic effect between them, not only can broad-spectrum and efficient antibacterial protection be provided, but also their respective characteristics can be utilized to enhance the overall antibacterial effect through synergistic effect, while bringing additional functions and user experience to the packaging material.

[0049] 3) The comparative analysis of the performance of the highly waterproof and environmentally friendly packaging paper box materials prepared in combination with Example 3 and Comparative Examples 3-4 shows that the silane coupling agent is composed of isopropyl trioleyl titanate and γ-(methacryloyloxy)propyl trimethoxy silane in a mass ratio of 3:4, and the synergistic effect between them is utilized to improve the comprehensive performance of the highly waterproof and environmentally friendly packaging paper box material.

[0050] 4) The performance comparison analysis of the highly waterproof and environmentally friendly packaging paper box material prepared in combination with Example 3 and Comparative Example 5 shows that the modified aqueous polyurethane emulsion successfully introduces di-terminal hydroxybutyl polydimethylsilane into the polyurethane segment by miniemulsion polymerization to obtain a modified aqueous polyurethane emulsion. The addition of di-terminal hydroxybutyl polydimethylsilane improves the compatibility between the polyurethane chain and the polyacrylate chain and reduces the degree of phase separation. By introducing the hydrophobic di-terminal hydroxybutyl polydimethylsilane, water molecules can be inhibited from penetrating from the surface of the highly waterproof and environmentally friendly packaging paper box material into the interior of the fabric, thereby improving the waterproofness of the needle-proof aqueous polyurethane coating.

[0051] 5) The performance comparison analysis of the highly waterproof and environmentally friendly packaging paper box material prepared in combination with Example 3 and Comparative Example 6 shows that the modified polylactic acid can effectively improve the toughness of the material by adding a modifier composed of tannic acid and phytic acid composite salt to the polylactic acid. This is because tannic acid and phytic acid composite salt can be used as plasticizers to increase the mobility between polymer chains, thereby reducing the brittleness of the material. Tannic acid and phytic acid composite salt can act as flame retardants in the material. Especially tannic acid, which is a natural flame retardant, can improve the thermal stability and flame retardancy of the material. The phytic acid composite salt in the modified polylactic acid has good water resistance, which helps to improve the waterproof performance of the overall material. The tannic acid in the modified polylactic acid undergoes a free radical grafting reaction with the sodium alginate in the carboxymethyl chitosan. This chemical reaction enhances the interaction between different layers and improves the adhesion between the layers. The grafting reaction increases the complexity of the internal structure of the material and forms a more stable network structure, which not only improves the overall performance of the material, but also helps to evenly disperse the applied pressure or impact force. Due to the above-mentioned characteristics of modified polylactic acid, it can effectively extend the service life of packaging cartons, making it more suitable for the needs of the food packaging industry.

[0052] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation modes of the present invention can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the scope of protection of the present application.

Claims

1. A highly waterproof and environmentally friendly packaging paper box material, characterized in that: The invention comprises a paperboard layer and a waterproof and antibacterial layer coated on the surface of the paperboard layer, wherein the thickness of the waterproof and antibacterial layer is 30-50 microns, and the waterproof and antibacterial layer is prepared by spraying a waterproof and antibacterial coating on the surface of the paperboard layer and curing the coating, wherein the waterproof and antibacterial coating comprises the following raw materials by weight: 100-110 parts of a modified waterborne polyurethane emulsion, 3-5 parts of carboxymethyl chitosan, 8-10 parts of a modified polylactic acid, 1-2 parts of a composite antibacterial agent, and 0.5-0.8 parts of a silane coupling agent, wherein the composite antibacterial agent consists of modified silver cerium doped titanium dioxide and peppermint oil.

2. A highly waterproof and environmentally friendly packaging paper box material according to claim 1, characterized in that: The mass ratio of the modified silver-cerium doped titanium dioxide to the peppermint oil is 3:

2.

3. The highly waterproof and environment-friendly packaging paper box material according to claim 1, characterized in that: The material of the paperboard layer is one of sack paper, kraft paper, kraft cardboard, boxboard and corrugated paper.

4. The highly waterproof and environment-friendly packaging paper box material according to claim 1, characterized in that: The thickness of the paperboard layer is 200-400 microns.

5. The highly waterproof and environment-friendly packaging paper box material according to claim 1, characterized in that: The preparation method of the modified aqueous polyurethane emulsion comprises the following steps: S51, according to the mass parts, 71 parts of di-terminal hydroxybutyl polydimethylsilane, 114 parts of butyl acrylate, 61 parts of styrene, 89 parts of polycaprolactone, 33 parts of isophorone diisocyanate, 3 parts of hydroxyethyl methacrylate, 1.8 parts of azobisisobutyronitrile, 0.5 parts of dibutyltin dilaurate and 10.5 parts of n-hexadecane were mixed uniformly to obtain a mixture; S52. Add the mixture into 300 parts of an aqueous emulsifier solution with a mass concentration of 6%, and then pre-emulsify at 3000r / min to obtain a crude emulsion, and then use a cell crusher to ultrasonically treat it in an ice-water bath for 40 minutes to obtain a monomer fine emulsion. Finally, stir the obtained monomer fine emulsion in a nitrogen atmosphere for 1.5 hours, transfer it to a three-necked flask, maintain the temperature at 72°C, and carry out a fine emulsion polymerization reaction in a nitrogen environment for 10 hours to obtain a modified waterborne polyurethane emulsion.

6. A highly waterproof and environment-friendly packaging paper box material according to claim 5, characterized in that: The emulsifier is 1-allyloxy-3-4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate.

7. A highly waterproof and environment-friendly packaging paper box material according to claim 1, characterized in that: The preparation method of the modified silver-cerium doped titanium dioxide comprises the following steps: S71. At room temperature, add 100 mL of tetra-n-butyl titanate to a solution consisting of 160 mL of ethanol and 30 mL of deionized water, and stir for 30 min to form solution A. S72, adding 1.5 g of silver nitrate and 12 g of cerium nitrate to a solution consisting of 100 mL of ethanol, 15 mL of acetic acid and 45 mL of water to form solution B; S73, adding solution B dropwise into solution A, stirring for 60 min, heating to 42° C., standing for 12 h, then centrifuging, washing, and drying at 80° C. for 12 h to obtain silver-cerium-doped titanium dioxide; S74, 0.8 g of γ-(methacryloyloxy)propyltrimethoxysilane was mixed with 70 g of ethanol and 8 g of water, and hydrolyzed for 4 h to obtain a mixture C; S75. Add the obtained silver-cerium-doped titanium dioxide to mixture C, then heat it to 43°C, stir it at 300 r / min for 250 min, and finally filter, wash, dry and grind it at 85°C to obtain modified silver-cerium-doped titanium dioxide with an average particle size of 40 nanometers.

8. The highly waterproof and environment-friendly packaging paper box material according to claim 1, characterized in that: The silane coupling agent is composed of isopropyl trioleyl titanate and gamma (methacryloyloxy) propyl trimethoxy silane in a mass ratio of 3:

4.

9. A highly waterproof and environment-friendly packaging paper box material according to claim 1, characterized in that: The preparation method of the modified polylactic acid comprises the following steps: S91, according to the mass parts, 131 parts of phytic acid solution with a mass concentration of 70%, 4.6 parts of citrulline, and 0.3 parts of genipin were mixed, the temperature was raised to 88°C and kept warm for 5 hours, purified with ethanol, filtered, and dried to obtain a phytic acid composite salt; S92. According to the weight ratio, 10 parts of tannic acid and 90 parts of phytic acid composite salt are mixed, and 900 parts of polylactic acid are added, and the mixture is mixed in a high-speed mixer to obtain modified polylactic acid.

10. A method for preparing a highly waterproof and environment-friendly packaging paper box material according to any one of claims 1 to 9, characterized in that: The following steps are involved: S101, uniformly stirring the modified waterborne polyurethane emulsion, carboxymethyl chitosan, modified polylactic acid, composite antibacterial agent and silane coupling agent according to their weight proportions to obtain a waterproof and antibacterial coating; S102, spraying the waterproof and antibacterial coating on the surface of the paperboard layer, and then drying it at 80-85° C. for 60-70 minutes to form a waterproof layer through a drying and curing process to obtain a highly waterproof and environmentally friendly packaging paper box material.

Citation Information

Patent Citations

  • Powerful smell removal antibiotic liquor

    CN101310775A

  • Organosilicon modified waterborne polyurethane emulsion and preparation method thereof

    CN105348476A

  • Waterproof and antibacterial coating

    CN106479303A

  • Waterproof and antibacterial corrugated carton

    CN109914148A

  • Cerium bromide doped titanium dioxide visible sterilization preparation

    CN112544632A

Cited By

  • Double-layer air filter paper with high interface adhesive force as well as preparation method and application of double-layer air filter paper

    CN120245554A