Composite membrane based on solid electrolyte as well as preparation method and application of composite membrane
Through the use of solid electrolyte composite membrane, the problems of shortage of lithium ore resources and high cost in lithium-ion battery recycling are solved, efficient separation and recycling of lithium ions are achieved, separation costs are reduced, and the mechanical properties and stability of the membrane are improved. .
Patent Information
- Application Number
- CN202411248412.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing lithium-ion battery recycling technology has problems of shortage of lithium ore resources and high costs. Torque metallurgy involves high temperature reactions and is seriously polluted. Hydrometallurgy requires high-cost design of membrane pore sizes to screen valuable metals.
Using a composite film based on solid electrolyte, a film composed of titanium aluminum lithium phosphate and polystyrene is used to separate lithium ions and divalent transition metal ions using size effect and hydrophobicity, reducing costs and improving mechanical properties.
It realizes efficient recycling of lithium elements in waste lithium-ion batteries, has excellent selectivity and permeability, reduces separation costs, and maintains stability under acid and alkaline conditions, making it suitable for industrial applications.
Smart Images

Figure CN118949714A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrodialysis recovery of waste lithium-ion batteries, and in particular to a composite membrane based on a solid electrolyte and a preparation method and application thereof. Background Art
[0002] Faced with the growing demand for energy consumption, the development of various renewable energy technologies has never stopped. The emergence of lithium-ion batteries has eased the pressure on large-scale energy storage systems and reduced environmental pollution. Lithium-ion batteries have become the main power source for various portable electronic devices, electric vehicles and emerging power grid systems due to their high energy density, long life and environmental friendliness. However, due to the uneven distribution of lithium mines and large-scale development and utilization, the price of lithium mines is also rising. In addition, a large number of waste batteries are piled up without treatment, and waste lithium batteries contain toxic precious metals and organic chemicals, causing immeasurable pollution to the environment. For example, most commercial anode materials contain toxic metals such as Co, Mn and Ni, which make the soil inactive after contact with the soil. Similarly, organic solvents such as LiPF6 in the electrolyte react with water to produce a large amount of toxic gases, which seriously pollute the air. Therefore, it is urgent to explore a sustainable and efficient way to recycle waste batteries.
[0003] In order to effectively alleviate the shortage and high cost of lithium ore resources, the main methods for recycling waste lithium-ion batteries are pyrometallurgy and hydrometallurgy. Since pyrometallurgy involves high-temperature reactions, it is bound to cause a lot of pollution while consuming a lot of energy, and this method cannot screen the valuable metals in the positive electrode materials of lithium-ion batteries. Hydrometallurgy is to treat the positive electrode materials with acid or alkali to obtain a leaching solution. The usual methods for separating and extracting the valuable metal ions in the leaching solution include membrane separation technology, chemical precipitation and other separation methods. In membrane separation technology, the performance of the membrane becomes the key to whether the ions can be extracted efficiently. However, it usually costs a lot of money to design the pore size and pore environment of the membrane. Obviously, although chemical modification can effectively separate ions, it still cannot meet the large-scale recycling of waste lithium-ion batteries.
[0004] In the solid electrolyte of lithium-ion batteries, the size of the ion transmission path in lithium aluminum titanium phosphate is just between the hydrated ion radius of lithium ions and divalent transition metal ions. Therefore, by utilizing the size effect between the solid electrolyte and the ions, the separation of valuable metals can be efficiently achieved, the lithium element in waste lithium-ion batteries can be recovered, and the high cost of designing membrane structure and pore size can be avoided. In terms of membrane preparation, polystyrene is used as a flexible frame, which greatly improves the mechanical properties of the solid electrolyte membrane. In addition, the hydrophobic nature of polystyrene also improves the tolerance of the composite membrane under acid and alkaline conditions. Summary of the invention
[0005] Technical problems to be solved: In view of the shortage and high cost of lithium ore resources in the existing technology, pyrometallurgy involves high-temperature reactions, which consumes a lot of energy and is bound to cause a lot of pollution. In addition, this method cannot screen the valuable metals in the positive electrode materials of lithium-ion batteries. It usually costs a lot of money to design the pore size and pore environment of the membrane. A composite membrane based on solid electrolyte and its preparation method and application are provided. The composite membrane can separate lithium ions and divalent transition metal ions in the leachate of waste lithium-ion batteries to achieve the recovery of lithium ions. It not only has excellent selectivity and permeability, but also greatly reduces the cost compared with other separation membranes.
[0006] A method for preparing a composite membrane based on a solid electrolyte, the preparation method comprising the following steps:
[0007] Step 1: In a beaker, weigh 2-3 parts of n-butyl titanate, 2-3 parts of phenyl phosphate, 0.1-1 parts of aluminum nitrate nonahydrate and 0.1-1 parts of lithium nitrate according to mass volume ratio, add them to 20 parts of tetrahydrofuran solution and mix evenly;
[0008] Step 2: Transfer the beaker containing the mixed solution obtained in step 1 to an oil bath to evaporate the solvent to obtain a sol-like substance;
[0009] Step 3: Transfer the sol-like substance remaining after evaporation to a muffle furnace for drying to obtain a precursor;
[0010] Step 4: Sintering the precursor in a tube furnace to prepare the solid electrolyte lithium aluminum titanium phosphate;
[0011] Step 5: Add 5-15 parts of polystyrene to 30-50 parts of tetrahydrofuran solution according to mass volume ratio and mix well;
[0012] Step 6: Add 0.5-1.5 parts of solid electrolyte to the mixed solution in step 5, and stir to obtain a white suspension;
[0013] Step 7: Add the white suspension dropwise onto the surface of the silicon wafer, and transfer it to a constant temperature box for evaporation after the added solution is evenly distributed on the surface of the silicon wafer;
[0014] Step 8: After evaporation, a white film is formed on the surface of the silicon wafer. The silicon wafer is placed in deionized water, and the white film falls off to obtain a composite film.
[0015] Furthermore, the ratio of n-butyl titanate: phenyl phosphoric acid: aluminum nitrate nonahydrate: lithium nitrate: tetrahydrofuran solution is 2.89:2.37:0.56:0.45:20 by mass.
[0016] Furthermore, in the first step, the mixing is performed by heating and stirring at 60° C., the stirring time is 5 to 6 hours, and the stirring speed is 600 rpm.
[0017] Furthermore, in the second step, the solvent evaporation temperature is 80° C., and the evaporation time is 6 to 8 hours.
[0018] Furthermore, in the third step, the muffle furnace drying temperature is 200° C., and the drying time is 6 to 12 hours.
[0019] Furthermore, in the fourth step, the precursor sintering temperature is 950-1100° C., the sintering time is 6-8 hours, and during the sintering process, the precursor is placed in a quartz boat for sintering, and the heating rate is 5° C. / min.
[0020] Furthermore, the mass volume ratio of the solid electrolyte: polystyrene: tetrahydrofuran solution is 1:10:40.
[0021] Furthermore, in the seventh step, the silicon wafer has a diameter of 2 inches, 1 mL of the white suspension is added dropwise, the evaporation temperature is 50-60° C., and the evaporation time is 6-12 hours.
[0022] The present application also discloses a composite membrane based on a solid electrolyte, which is composed of a lithium-ion battery solid electrolyte and a self-supporting flexible frame; wherein the solid electrolyte loading accounts for 10%, the flexible frame loading accounts for 90%, the membrane thickness is 9-11mm, the solid electrolyte is lithium aluminum titanium phosphate LATP prepared by a sol-gel method, and the component of the self-supporting flexible frame is polystyrene PS.
[0023] The present application also discloses the use of a composite membrane based on a solid electrolyte in extracting lithium from waste lithium-ion batteries. The composite membrane screens valuable metal ions through a solid electrolyte to extract lithium from a leachate of waste lithium-ion batteries.
[0024] Principle explanation: The solid electrolyte contains vacancies and transmission channels for lithium ions. Driven by the electric field, lithium ions enter the solid electrolyte to occupy the vacancies. When the electric field strength supports the maximum migration barrier of lithium ions, lithium ions realize vacancy conduction in the solid electrolyte and eventually reach from one side of the solution to the other, thereby realizing the separation of lithium ions in the leachate of waste lithium-ion batteries.
[0025] Beneficial effects:
[0026] 1. The transmission channel of the solid electrolyte has excellent separation performance for valuable metals due to the size effect. Compared with conventional commercial anion / cation exchange membranes, the solid electrolyte composite membrane provided by the present application has the separation performance of ions of the same valence, and is used to extract lithium from the leachate of waste lithium-ion batteries;
[0027] 2. Compared with the separation membrane based on pore design, the solid electrolyte composite membrane provided by the present application has lower cost, and polystyrene has higher ductility and hydrophobicity, which increases the mechanical properties of the composite membrane and tolerance in acid / alkaline solutions;
[0028] 3. Compared with other solid electrolytes, the size of the lithium ion transmission path in the lithium aluminum titanium phosphate structure is more consistent with the size of hydrated lithium ions. The required raw materials are all commercial chemicals with low cost. In addition, the preparation process of this method is simple and safe to operate, and it is easy to realize industrialization.
[0029] 4. A solid electrolyte, lithium aluminum titanium phosphate, is prepared by a sol-gel method, and then mixed with polystyrene to prepare a solid electrolyte composite membrane by drop coating. The solid electrolyte composite membrane provided by the present application involves a polystyrene self-supporting frame that is hydrophobic, so that the composite membrane has good tolerance and stability;
[0030] 5. The preparation method of the solid electrolyte composite membrane provided in this application has the advantages of simple and safe preparation process, and is easy to achieve large-scale preparation. After 3 hours of testing, the ICP test results showed that the lithium ion concentration on the solution collection side of the solid electrolyte membrane rose to 0.879 mg mL -1 , while the concentration of cobalt ions has basically not changed. Neither lithium ions nor cobalt ions pass through the solution collection side of the PS membrane. Therefore, the solid electrolyte composite membrane has a high ion selectivity of 109 and has good application prospects;
[0031] 6. In the 3-hour long cycle test, the solid electrolyte membrane still maintains high ion selectivity, indicating that it has a good service life. Therefore, using the most common and inexpensive polystyrene material as the frame, the solid electrolyte composite membrane has excellent stability and mechanical properties, and has good application prospects in industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The solid electrolyte Li in the embodiment of this application 1.3 Al 0.3 Ti 1.7 SEM images of (PO4)3 materials, where a is a high-magnification SEM image of the solid electrolyte and b is a low-magnification SEM image of the solid electrolyte;
[0033] Figure 2 In the embodiment of this application, Li 1.3 Al 0.3 Ti 1.7 XRD pattern of (PO4)3 material;
[0034] Figure 31 are SEM images of the solid electrolyte composite membrane and the PS membrane prepared by the drop coating method in the examples and comparative examples of the present application, wherein a is the SEM of the solid electrolyte composite membrane in the example, and b is the SEM surface image of the PS membrane in the comparative example;
[0035] Figure 4 It is an electrochemical LSV test model diagram of single solution ion conductivity of the embodiments and comparative examples of the present application;
[0036] Figure 5 It is an electrochemical IT test model diagram of the single solution separation performance of the embodiments and comparative examples of the present application;
[0037] Figure 6 The electrochemical LSV test data of the examples and comparative examples of the present application, wherein a is a surface image of the solid electrolyte composite membrane, and b is a surface image of the PS membrane;
[0038] Figure 7 The electrochemical IT test data of the embodiments and comparative examples of the present application. DETAILED DESCRIPTION
[0039] The following are only embodiments of the present invention, and are not intended to limit the scope of the present invention. The present invention can be implemented in different forms, and all contents made using the contents of the present invention specification are included in the scope of patent protection of the present invention. The embodiments are provided to make the contents disclosed in the present invention more thorough and comprehensive.
[0040] Unless otherwise specified, all numbers appearing in the specification and claims of this application, such as active components, temperature, time, pressure, etc., should not be understood as absolutely precise values. Due to the standard deviation of the measurement technology, the measured values inevitably have certain experimental errors.
[0041] Unless otherwise specified, the raw materials and reagents in the examples of this application can be purchased through commercial channels. The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0042] Example 1
[0043] A method for preparing a composite membrane based on a solid electrolyte, the preparation method comprising the following steps:
[0044] Step 1: In a beaker, weigh n-butyl titanate, phenyl phosphoric acid, aluminum nitrate nonahydrate and lithium nitrate according to the mass ratio of n-butyl titanate: phenyl phosphoric acid: aluminum nitrate nonahydrate: lithium nitrate: tetrahydrofuran solution = 2.89:2.37:0.56:0.45:20, add them to the tetrahydrofuran solution, heat and stir at 60°C for 5 to 6 hours, and the stirring speed is 600 rpm;
[0045] Step 2: Transfer the beaker containing the mixed solution obtained in step 1 to an oil bath to evaporate the solvent to obtain a sol-like substance. The evaporation temperature is 80°C and the evaporation time is 6 to 8 hours.
[0046] Step 3: Transfer the sol-like substance remaining after evaporation to a muffle furnace for drying to obtain a precursor. The drying temperature of the muffle furnace is 200°C and the drying time is 6 to 12 hours.
[0047] Step 4: Sinter the precursor in a tube furnace to prepare a solid electrolyte lithium aluminum titanium phosphate. The precursor sintering temperature is 950-1100°C and the sintering time is 6-8h. During the sintering process, the precursor is placed in a quartz boat for sintering at a heating rate of 5°C / min.
[0048] Step 5: The mass volume ratio of the solid electrolyte: polystyrene: tetrahydrofuran solution is 1:10:40. After sealing the aqueous solution, transfer it to a heated stirring table, heat it to 60°C, and stir it at a speed of 600 rpm;
[0049] Step 6: Add 1 part of the solid electrolyte to the mixed solution in step 5, and stir at 60°C for 6-8h to obtain a solid electrolyte composite membrane solution;
[0050] Step 7: Use a pipette to drop the white suspension onto the surface of the silicon wafer. After the solution is evenly distributed on the surface of the silicon wafer, transfer it to a constant temperature box for evaporation. The silicon wafer has a diameter of 2 inches. 1 mL of the white suspension is added. The evaporation temperature is 50-60°C and the evaporation time is 6-12 hours.
[0051] Step 8: After evaporation, a white film is formed on the surface of the silicon wafer. The silicon wafer is placed in deionized water, and the white film falls off to obtain a composite membrane based on a solid electrolyte.
[0052] Comparative Example 1
[0053] The polystyrene (PS) membrane of the present comparative example does not contain the solid electrolyte lithium aluminum titanium phosphate active component, specifically:
[0054] This comparative example is based on the same method as the embodiment, except that the separation membrane does not contain solid electrolyte and only includes a polystyrene flexible frame, and the membrane preparation process is the same as the embodiment.
[0055] Figure 1 It's Li 1.3 Al 0.3 Ti 1.7 SEM images (a) and (b) of (PO4)3 material, where a is a high-magnification SEM image of the solid electrolyte and b is a low-magnification SEM image of the solid electrolyte. The particle size of the solid electrolyte powder is 400nm.
[0056] Figure 2 It's Li1.3 Al 0.3 Ti 1.7 The XRD pattern of (PO4)3 material shows that Li 1.3 Al 0.3 Ti 1.7 (PO4)3 material.
[0057] Figure 3 The SEM surface images of the solid electrolyte composite membrane (a) and the PS membrane (b) prepared by the drop coating method.
[0058] Figure 4 It is an electrochemical test model diagram of single solution ion conductivity. The test membrane is sandwiched between two electrolytic cells, with leachate on the left and right sides. AgCl electrodes are used on both sides of the solution phase and are connected to a chemical workstation; the working electrode of the chemical workstation is connected to the AgCl electrode in the leachate, while the auxiliary electrode and reference electrode are connected to the AgCl electrode in the leachate on the other side.
[0059] Figure 5 This is an electrochemical test model diagram of solution separation performance. The test membrane is sandwiched between two electrolytic cells, with the leachate on the left and ultrapure water on the right. AgCl electrodes are used on both sides of the solution phase and are connected to a chemical workstation; the working electrode of the chemical workstation is connected to the AgCl electrode in the leachate, while the auxiliary electrode and reference electrode are connected to the AgCl electrode in the ultrapure water.
[0060] Figure 6 The linear sweep voltammetry test is used, and the specific steps are as follows:
[0061] use Figure 1 In the model, 35 mL of 0.1 M LiCl solution was added to both sides, the open circuit voltage was set to 0 V, and the final value voltage was set to 0.2 V. The scan rate was 0.005 V / s, the sampling interval was 0.001 V, and the iV curve was obtained. Its slope represents the conductivity value. The above operation was repeated by replacing the CoCl2 solution, and the iV curve was obtained as well. Figure 6 After the above test is completed, replace the PS film and perform the LSV test according to the same steps as above to obtain the iV curve, as shown in Figure 6 As shown in b. The test results show that Li + and Co 2+ It can pass through the composite membrane, but not the PS membrane. And the conductivity calculated from the slope can well explain the Li + The flux is much greater than that of Co 2+ , showing good separation performance.
[0062] Figure 7It is an ampere it test, and its specific steps are as follows:
[0063] use Figure 2 For the model in , 35 mL of 0.1 M LiCl solution was added to the left side and 35 mL of ultrapure water was added to the right side. The initial voltage was set to 0.1 V and the time was set to 3 h. The it curve was obtained by testing. During the test, 1 mL of solution on the ultrapure water side was taken for inductively coupled plasma (ICP) test every 0.5 h. The CoCl2 solution was replaced and the above operation was repeated. After the above test was completed, the PS membrane was replaced and the ampere it test was performed according to the same steps as above to obtain the it curve, and 1 mL of solution on the ultrapure water side was taken for ICP test.
[0064] Table 1 is the ICP test data results after 3 hours of amperometric test. According to the ICP test results, we can further see that the composite membrane has good separation performance of monovalent and divalent ions, and the membrane also has excellent stability.
[0065] Table 1 ICP test data of embodiments and comparative examples
[0066]
[0067] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite membrane based on a solid electrolyte, characterized in that: The preparation method comprises the following steps: Step 1: In a beaker, weigh 2-3 parts of n-butyl titanate, 2-3 parts of phenyl phosphate, 0.1-1 parts of aluminum nitrate nonahydrate and 0.1-1 parts of lithium nitrate according to mass volume ratio, add them to 20 parts of tetrahydrofuran solution and mix evenly; Step 2: Transfer the beaker containing the mixed solution obtained in step 1 to an oil bath to evaporate the solvent to obtain a sol-like substance; Step 3: transferring the sol-like substance remaining after evaporation to a muffle furnace for drying to obtain a precursor; Step 4: Sintering the precursor in a tube furnace to prepare the solid electrolyte lithium aluminum titanium phosphate; Step 5: Add 5-15 parts of polystyrene to 30-50 parts of tetrahydrofuran solution according to mass volume ratio and mix well; Step 6: Add 0.5-1.5 parts of solid electrolyte to the mixed solution in step 5, stir at 60°C for 6-8h to obtain a solid electrolyte composite membrane solution, and the stirring speed is 600 rpm; Step 7: Add the white suspension dropwise onto the surface of the silicon wafer, and transfer it to a constant temperature box for evaporation after the added solution is evenly distributed on the surface of the silicon wafer; Step 8: After evaporation, a white film is formed on the surface of the silicon wafer. The silicon wafer is placed in deionized water, and the white film falls off to obtain a composite membrane based on a solid electrolyte.
2. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: The mass ratio of n-butyl titanate: phenyl phosphoric acid: aluminum nitrate nonahydrate: lithium nitrate: tetrahydrofuran solution is 2.89:2.37:0.56:0.45:
20.
3. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: The mixing in the first step is performed by heating and stirring at 60° C., the stirring time is 5 to 6 hours, and the stirring speed is 600 rpm.
4. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: In the second step, the solvent evaporation temperature is 80° C. and the evaporation time is 6 to 8 hours.
5. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: In the third step, the muffle furnace drying temperature is 200° C., and the drying time is 6 to 12 hours.
6. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: In the fourth step, the precursor sintering temperature is 950-1100° C., and the sintering time is 6-8 hours. During the sintering process, the precursor is placed in a quartz boat for sintering, and the heating rate is 5° C. / min.
7. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: The solid electrolyte: polystyrene: tetrahydrofuran solution is in a mass volume ratio of 1:10:
40. The aqueous solution is sealed and transferred to a heated stirring table, heated to 60° C., and the stirring speed is 600 rpm.
8. The method for preparing a composite membrane based on a solid electrolyte according to claim 1, characterized in that: In the seventh step, the diameter of the silicon wafer is 2 inches, 1 mL of the white suspension is added dropwise, the evaporation temperature is 50-60° C., and the evaporation time is 6-12 hours.
9. A composite membrane based on a solid electrolyte prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The composite membrane based on solid electrolyte is composed of a lithium-ion battery solid electrolyte and a self-supporting flexible frame; the solid electrolyte loading accounts for 10%, the flexible frame loading accounts for 90%, the membrane thickness is 9-11 mm, the solid electrolyte is lithium aluminum titanium phosphate LATP prepared by a sol-gel method, and the self-supporting flexible frame is composed of polystyrene PS.
10. An application of the composite membrane based on solid electrolyte according to claim 9 in extracting lithium from waste lithium-ion batteries, characterized in that: The composite membrane screens valuable metal ions through solid electrolytes and extracts lithium from the leachate of waste lithium-ion batteries.