Powder reinforcing agent for normal-temperature hardening as well as preparation method and use method of powder reinforcing agent

By combining the powder reinforcement agent hardened at room temperature, with silicate inorganic binder and liquid curing agent, the problems of high odor, high cost and heating and hardening during the use of the binder in the prior art are solved, and high strength is achieved , low-cost sand production simplifies the process and improves production efficiency and safety.

CN118950928APending Publication Date: 2024-11-15SHARED NEW MATERIALS (SHANDONG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010742.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The binders in the existing casting field have problems such as high odor, high cost, great influence on humidity, and complex curing agent preparation process during use. In particular, inorganic binders need to be heated and hardened, resulting in low strength and high production costs.

Method used

Provide a powder reinforcement agent for hardening at room temperature, including microsilicon fume, phosphate compounds, cellulose modifiers, inorganic salt oxide powders, alcohol amine compounds and borate compounds, which are prepared evenly by stirring and used for The silicate inorganic binder and liquid curing agent are mixed to achieve sand production that is hardened at room temperature.

Benefits of technology

The amount of adhesive and curing agent is added is reduced, the strength and surface accuracy of the sand type is improved, the process is simplified, the production cost is reduced, and the heating and hardening is not required, which improves production efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964279600000091
    Figure BDA0004964279600000091
Patent Text Reader

Abstract

The invention relates to the technical field of binders, and provides a powder reinforcing agent for normal-temperature hardening as well as a preparation method and a use method of the powder reinforcing agent for normal-temperature hardening. Comprising the following components in percentage by weight: 41.5%-65% of micro-silica fume, 8%-22% of a phosphate compound, 10%-25% of a cellulose modifier, 2%-8% of inorganic salt oxide powder, 0.4%-2% of an alcohol amine compound and 0.2%-2% of a borate compound. The silicon dioxide content of the micro-silica fume can be 85%-99%; the phosphate compound is one or more of disodium hydrogen phosphate, sodium hexametaphosphate, sodium tripolyphosphate and aluminum dihydrogen phosphate; the inorganic salt oxide powder is one or more of calcium oxide, aluminum oxide and magnesium oxide. When the sand mold is manufactured, the method has the advantages that the addition amount of a binder and a curing agent is small, the strength of the sand mold (core) is high, the curing speed is high, the surface precision of the sand mold (core) is high, and the production process is simple and environmentally friendly; the method can be used for normal-temperature hardening of casting inorganic binders and traditional casting manual modeling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and more particularly to a powder reinforcing agent for room temperature hardening of adhesives. Background Art

[0002] At present, the types of binders used for bonding of molding sand in the foundry field at home and abroad mainly include furan resin, phenolic resin, inorganic binder, etc. These three types of binders are used in different scenarios due to their different characteristics. Among them, furan resin has the characteristics of high molding sand strength and good sand regeneration performance. It can be used in the production of sand molds (cores) for cast iron parts and non-ferrous metal parts, but it emits a strong odor when used and the strength of the molding sand is greatly affected by humidity; the sand mold (core) printed by phenolic resin has high strength after drying and high high-temperature residual strength after casting. It can be used for the production of steel castings, but it has the disadvantages of high raw material cost, high resin addition, high VOC emissions, and difficulty in regenerating old sand. Silicate inorganic binders have the advantages of high sand mold (core) strength, little influence by humidity, low raw material cost, no odor and VOC emission, etc., which make up for the disadvantages of using organic binders such as furan resin and phenolic resin. However, the liquid curing agent used with the inorganic binder needs to be heated and hardened during use, otherwise its strength is low and cannot be used normally. In addition, the preparation process of the curing agent used with the inorganic binder is complicated and the production cost is high. Summary of the invention

[0003] The present invention aims at the existing problems and provides a powder reinforcing agent product used in combination with a silicate inorganic binder and a liquid curing agent. The powder reinforcing agent product is mixed with the silicate inorganic binder and the matching liquid curing agent to produce a sand mold with the advantages of less binder and curing agent addition, high sand mold (core) strength, fast curing speed, high sand mold (core) surface precision, simple production process, environmental protection, etc. The powder reinforcing agent can be used not only for casting silicate inorganic binder hardening at room temperature, but also for traditional casting manual molding.

[0004] In order to achieve its purpose, the present invention provides the following technical solutions: On the one hand, the purpose of the present invention is to provide a powder reinforcing agent for room temperature hardening, which comprises the following components and contents by weight percentage:

[0005] Microsilica fume 41.5%-65%, phosphate compounds 8%-22%, cellulose modifier 10%-25%, inorganic salt oxide powder 2%-8%, alcohol amine compounds 0.4%-2%, borate compounds 0.2%-2%;

[0006] The silicon dioxide content of the microsilica fume can be 85%-99%; the phosphate compound is one or more of disodium hydrogen phosphate, sodium hexametaphosphate, sodium tripolyphosphate, and aluminum dihydrogen phosphate; the inorganic salt oxide powder is one or more of calcium oxide, aluminum oxide, and magnesium oxide.

[0007] In one embodiment, preferably, the content of silicon dioxide is ≥90%, and the mesh size range used is 70-140 mesh.

[0008] In one embodiment, preferably, the mesh size range of the phosphate compound used is 100-140 mesh.

[0009] In one embodiment, preferably, the mesh size range of the inorganic salt oxide powder is 90-160 mesh.

[0010] Furthermore, the cellulose modifier is one or more of hydroxypropyl methylcellulose, calcium lignin sulfonate, sodium lignin sulfonate, sodium carboxymethyl cellulose, and hydroxyethyl methylcellulose, and the mesh size range is 80-150 meshes.

[0011] Furthermore, the alcoholamine compound is one or more of diethanolisopropanolamine, diisopropanolamine, and triisopropanolamine, and the mesh size range used is 70-140 meshes.

[0012] Furthermore, the borate compound is one or more of sodium tetraborate and potassium tetraborate, and the mesh size range used is 80-150 mesh.

[0013] On the other hand, the object of the present invention is to provide a method for preparing a powder reinforcing agent for room temperature hardening, comprising the following steps:

[0014] S1: Put microsilica fume, phosphate compound and cellulose modifier into a closed stirring kettle in sequence and stir evenly;

[0015] S2: Add inorganic salt oxide powder and stir to mix evenly;

[0016] S3: adding an amine compound and a borate compound, and continuing to stir to mix them evenly to obtain a powder reinforcing agent for room temperature curing.

[0017] The present invention also provides a method for using a powder reinforcing agent that hardens at room temperature. According to the weight of the molding sand, the powder reinforcing agent is added in an amount of 1%-3% of the weight of the sand, the curing agent is added in an amount of 0.8%-2% of the weight of the sand, and the molding sand is mixed evenly in sequence. The inorganic binder is added in an amount of 2%-2.4% of the weight of the sand, and the molding sand can be hardened at room temperature. The beneficial effects of the present invention are:

[0018] The powder enhancer and preparation method thereof provided by the present invention have the following advantages and beneficial effects:

[0019] The powder enhancer of the present invention is in a solid state, and the raw materials used are all in powder form, the process configuration process is simple, easy to operate, and the production efficiency is high. It is also convenient to store and has a long shelf life. The powder enhancer of the present invention is stable in state, non-volatile, has no irritating odor, and is highly safe for production and on-site use. The several powder raw material components in the powder enhancer of the present invention have different particle size specifications, and when mixed with molding sand, they can play a grinding aid effect, so that the surface density of the prepared sand mold is better and the precision is higher.

[0020] The introduction of the reinforcing agent of the present invention can effectively reduce the amount of binder and curing agent added when making sand molds, the amount of inorganic binder added can be reduced by 10%-20%, and the amount of curing agent added can be reduced by 20%-30%. After the powder reinforcing agent and the liquid curing agent of the present invention are uniformly mixed with the molding sand in sequence, the printed or manually prepared sand mold can be hardened at room temperature after inkjet printing or manual molding is performed, and no additional heating is required to promote hardening, which can reduce the production cost by 3%-12%, but the strength of the sand mold (core) is improved by 15%-20%.

[0021] By adding microsilica fume, sodium tripolyphosphate and inorganic salt oxide to the powder enhancer of the present invention, the demolding time of the sand mold (core) during printing or molding can be shortened by 30%-36%; by adding cellulose modifier, amine compound, borate compound and other materials to the powder enhancer of the present invention, the room temperature strength of the printed or molded sand mold (core) can be increased by 20%-35%. DETAILED DESCRIPTION

[0022] To facilitate understanding of the present invention, the present invention will be described more fully below.

[0023] Implementation case 1:

[0024] This embodiment provides a powder reinforcing agent for room temperature curing. The total weight of raw materials is 100 kg, and the components are as follows by weight percentage:

[0025] 41.5% microsilica (silicon dioxide content is 90%, using powdered raw materials with a mesh size of 100 mesh), 22% disodium hydrogen phosphate (using powdered raw materials with a mesh size of 120 mesh), 24.9% hydroxypropyl methylcellulose (using powdered raw materials with a mesh size of 80 mesh), 7.9% alumina powder (using powdered raw materials with a mesh size of 110 mesh), 1.9% triisopropanolamine (using powdered raw materials with a mesh size of 80 mesh), 1.8% sodium tetraborate (using powdered raw materials with a mesh size of 150 mesh).

[0026] The embodiment of the present invention also provides a method for preparing a powder reinforcing agent for room temperature hardening. The raw materials of the above scheme are prepared according to the following method:

[0027] S1: 41.5% microsilica fume, 22% disodium hydrogen phosphate and 24.9% hydroxypropyl methylcellulose are sequentially put into a closed stirring kettle and stirred evenly;

[0028] S2: Add 7.9% alumina powder and stir to mix evenly;

[0029] S3: Finally, add 1.9% triisopropanolamine and 1.8% sodium tetraborate and continue stirring to mix them evenly to obtain a powder reinforcing agent product for room temperature hardening.

[0030] The powder reinforcing agent product for room temperature hardening is prepared by adding 1.8% (total sand ratio) of the product and 1.3% (total sand ratio) of the curing agent in sequence with 100-140 mesh printing silica sand and stirring and mixing them evenly, and then adding 2.4% silicate inorganic binder (total sand ratio) and stirring and mixing evenly, and then hardening can be carried out at room temperature to produce sand molds.

[0031] At the same time, a control group experiment was carried out. In the control group experiment, the invented curing agent was added at 1.8% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 2.8% silicate inorganic binder (total sand ratio) was added and mixed evenly. During the hardening process, heating at 160 degrees was required to produce sand molds.

[0032] The sand molds made by the product of the present invention and the sand molds made by the control group method were tested for their room temperature tensile strength, 1000°C high temperature tensile strength, and demolding time.

[0033] Implementation case 2:

[0034] This embodiment provides a powder reinforcing agent for room temperature curing. The total weight of raw materials is 100 kg, and the components are as follows by weight percentage:

[0035] 60.1% microsilica fume (silicon dioxide content is 95%, using a powdered raw material with a mesh size of 90 mesh), 12% sodium hexametaphosphate (using a powdered raw material with a mesh size of 100 mesh), 25% calcium lignin sulfonate (using a powdered raw material with a mesh size of 100 mesh), 2% magnesium oxide powder (using a powdered raw material with a mesh size of 90 mesh), 0.4% diethanol isopropanolamine (using a powdered raw material with a mesh size of 70 mesh), and 0.5% potassium tetraborate (using a powdered raw material with a mesh size of 80 mesh).

[0036] The embodiment of the present invention also provides a method for preparing a powder reinforcing agent for room temperature hardening. The raw materials of the above scheme are prepared according to the following method:

[0037] S1: 60.1% microsilica fume, 12% sodium hexametaphosphate and 25% calcium lignin sulfonate are sequentially put into a closed stirring kettle and stirred evenly;

[0038] S2: Add 2% magnesium oxide powder and stir to mix evenly;

[0039] S3: Finally, add 0.4% of diethanol isopropanolamine and 0.5% of potassium tetraborate and continue stirring to mix them evenly to obtain a powder reinforcing agent product for room temperature hardening.

[0040] The prepared powder reinforcing agent product for room temperature hardening is added in an amount of 1.6% (total sand ratio) and a curing agent in an amount of 1.5% (total sand ratio) and mixed with 100-140 mesh printing silica sand in sequence, and then 2.5% silicate inorganic binder (total sand ratio) is added and stirred and mixed evenly, and then it can be hardened at room temperature to produce sand molds.

[0041] At the same time, a control group experiment was carried out. In the control group experiment, the invented curing agent was added at 1.9% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 2.9% silicate inorganic binder (total sand ratio) was added and mixed evenly. During the hardening process, heating at 140 degrees was required to produce sand molds.

[0042] The sand molds made by the product of the present invention and the sand molds made by the control group method were tested for their room temperature tensile strength, 1000°C high temperature tensile strength, and demolding time.

[0043] Implementation Case 3

[0044] This embodiment provides a powder reinforcing agent for room temperature curing. The total weight of raw materials is 100 kg, and the components are as follows by weight percentage:

[0045] 64% microsilica fume (silicon dioxide content is 98%, using a powdered raw material with a mesh number of 110 mesh), 21.3% sodium tripolyphosphate (using a powdered raw material with a mesh number of 110 mesh), 10% sodium lignin sulfonate (using a powdered raw material with a mesh number of 120 mesh), 2.5% calcium oxide powder (using a powdered raw material with a mesh number of 100 mesh), 2% diisopropanolamine (using a powdered raw material with a mesh number of 90 mesh), and 0.2% potassium tetraborate (using a powdered raw material with a mesh number of 90 mesh).

[0046] The embodiment of the present invention also provides a method for preparing a powder reinforcing agent for room temperature hardening. The raw materials of the above scheme are prepared according to the following method:

[0047] S1: 64% microsilica fume, 21.3% sodium tripolyphosphate and 10% sodium lignin sulfonate are sequentially put into a closed stirring kettle and stirred evenly;

[0048] S2: Add 2.5% calcium oxide powder and stir to mix evenly;

[0049] S3: Finally, add 2% of diisopropanolamine and 0.2% of potassium tetraborate and continue stirring to mix them evenly to obtain a powder reinforcing agent product for room temperature hardening.

[0050] The powder reinforcing agent product prepared for room temperature hardening is added in an amount of 2.0% (total sand ratio) and a curing agent in an amount of 1.2% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 2.2% silicate inorganic binder (total sand ratio) is added and stirred and mixed evenly, and then it can be hardened at room temperature to produce sand molds.

[0051] At the same time, a control group experiment was carried out. In the control group experiment, the invented curing agent was added at 1.8% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 3% silicate inorganic binder (total sand ratio) was added and mixed evenly. During the hardening process, heating at 120 degrees was required to produce sand molds.

[0052] The sand molds made by the product of the present invention and the sand molds made by the control group method were tested for their room temperature tensile strength, 1000°C high temperature tensile strength, and demolding time.

[0053] Implementation Case 4

[0054] This embodiment provides a powder reinforcing agent for room temperature curing. The total weight of raw materials is 100 kg, and the components are as follows by weight percentage:

[0055] 65% microsilica (silicon dioxide content is 96%, using powdered raw materials with a mesh size of 80 mesh), 8% aluminum dihydrogen phosphate (using powdered raw materials with a mesh size of 140 mesh), 21.8% sodium carboxymethyl cellulose (using powdered raw materials with a mesh size of 90 mesh), 3% alumina powder (using powdered raw materials with a mesh size of 120 mesh), 1.2% triisopropanolamine (using powdered raw materials with a mesh size of 100 mesh), and 1% sodium tetraborate (using powdered raw materials with a mesh size of 100 mesh).

[0056] The embodiment of the present invention also provides a method for preparing a powder reinforcing agent for room temperature hardening. The raw materials of the above scheme are prepared according to the following method:

[0057] S1: 65% microsilica fume, 8% aluminum dihydrogen phosphate and 21.8% sodium carboxymethyl cellulose are sequentially put into a closed stirring kettle and stirred evenly;

[0058] S2: Add 3% of aluminum oxide powder and stir to mix evenly;

[0059] S3: Finally, add 1.2% triisopropanolamine and 1% sodium tetraborate and continue stirring to mix them evenly to obtain a powder reinforcing agent product for room temperature hardening.

[0060] The powder reinforcing agent product for room temperature hardening is prepared by adding 2.2% (total sand ratio) of the product and 0.8% (total sand ratio) of the curing agent in sequence with 100-140 mesh printing silica sand and stirring and mixing them evenly, and then adding 2.3% silicate inorganic binder (total sand ratio) and stirring and mixing evenly, and then hardening can be carried out at room temperature to produce sand molds.

[0061] At the same time, a control group experiment was carried out. In the control group experiment, the invented curing agent was added at 1.8% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 2.9% silicate inorganic binder (total sand ratio) was added and mixed evenly. During the hardening process, heating at 150 degrees was required to produce a sand mold.

[0062] The sand molds made by the product of the present invention and the sand molds made by the control group method were tested for their room temperature tensile strength, 1000°C high temperature tensile strength, and demolding time.

[0063] Implementation Case 5

[0064] This embodiment provides a powder reinforcing agent for room temperature curing. The total weight of raw materials is 100 kg, and the components are as follows by weight percentage:

[0065] 64.3% microsilica (silicon dioxide content is 95%, using a powdered raw material with a mesh size of 70 mesh), 11.4% sodium tripolyphosphate (using a powdered raw material with a mesh size of 130 mesh), 13.4% hydroxyethyl methylcellulose (using a powdered raw material with a mesh size of 140 mesh), 8% magnesium oxide powder (using a powdered raw material with a mesh size of 150 mesh), 0.9% diethanol isopropanolamine (using a powdered raw material with a mesh size of 110 mesh), and 2% sodium tetraborate (using a powdered raw material with a mesh size of 120 mesh).

[0066] The embodiment of the present invention also provides a method for preparing a powder reinforcing agent for room temperature hardening. The raw materials of the above scheme are prepared according to the following method:

[0067] S1: 64.3% microsilica fume, 11.4% sodium tripolyphosphate and 13.4% hydroxyethyl methyl cellulose are sequentially put into a closed stirring kettle and stirred evenly;

[0068] S2: Add 8% magnesium oxide powder and stir to mix evenly;

[0069] S3: Finally, add 0.9% of diethanol isopropanolamine and 2% of sodium tetraborate and continue stirring to mix them evenly to obtain a powder reinforcing agent product for silicate inorganic binder.

[0070] The prepared powder reinforcing agent product for room temperature hardening is added in an amount of 2.5% (total sand ratio) and a curing agent in an amount of 1.2% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 2.1% silicate inorganic binder (total sand ratio) is added and stirred and mixed evenly, and then it can be hardened at room temperature to produce sand molds.

[0071] At the same time, a control group experiment was carried out. In the control group experiment, the invented curing agent was added at 1.8% (total sand ratio) and mixed evenly with 100-140 mesh printing silica sand, and then 3% silicate inorganic binder (total sand ratio) was added and mixed evenly. During the hardening process, heating at 200 degrees was required to produce a sand mold.

[0072] The sand molds made by the product of the present invention and the sand molds made by the control group method were tested for their room temperature tensile strength, 1000°C high temperature tensile strength, and demolding time.

[0073] The test results of the product of the embodiment of the present invention and the product of the comparison group were compared, as shown in Table 1:

[0074] Table 1 Comparison of sand mold properties of the products of the present invention and the comparative examples

[0075]

[0076] As can be seen from the embodiments, in the present invention, the powder enhancer components are all powdered solids, the configuration process is simple, easy to operate, and the production efficiency is high; the powder enhancer of the present invention is stable, non-volatile, has no irritating odor, and is highly safe for production and on-site use. The enhancer of the present invention is added in a small amount during the molding sand manufacturing process, accounting for about 1.0%-3.0% of the specific gravity of the molding sand, which reduces the amount of curing agent and binder added, reduces the odor and environmental safety hazards at the production site, and does not require heating equipment, saving the cost of use, and the strength is increased by 15%-20%, which can increase the normal temperature strength of the printed or molded sand mold (core) by 20%-35%. The demolding time of the sand mold (core) during printing or molding can be shortened and increased by 30%-36%. At the same time, the surface density of the prepared sand mold is better and the dimensional accuracy is higher.

[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A powder reinforcing agent for room temperature hardening, characterized in that: By weight percentage, it includes the following components and contents: 41.5%-65% microsilica fume, 8%-22% phosphate compound, 10%-25% cellulose modifier, 2%-8% inorganic salt oxide powder, 0.4%-2% alcoholamine compound, 0.2%-2% borate compound; the silicon dioxide content of the microsilica fume can be 85%-99%; The phosphate compound is one or more of disodium hydrogen phosphate, sodium hexametaphosphate, sodium tripolyphosphate, and aluminum dihydrogen phosphate; The inorganic salt oxide powder is one or more of calcium oxide, aluminum oxide and magnesium oxide.

2. A powder reinforcing agent for room temperature hardening according to claim 1, characterized in that: Preferably, the content of silicon dioxide is ≥90%, and the mesh size range used is 70-140 mesh.

3. A powder reinforcing agent for room temperature hardening according to claim 1, characterized in that: The mesh size range of the phosphate compound is 100-140 mesh.

4. The powder reinforcing agent for room temperature hardening according to claim 1, characterized in that: The cellulose modifier is one or more of hydroxypropyl methylcellulose, calcium lignin sulfonate, sodium lignin sulfonate, sodium carboxymethyl cellulose, and hydroxyethyl methylcellulose, and the mesh size range is 80-150 meshes.

5. The powder reinforcing agent for room temperature hardening according to claim 1, characterized in that: The mesh size of the inorganic salt oxide powder is in the range of 90-160 meshes.

6. The powder reinforcing agent for room temperature hardening according to claim 1, characterized in that: The alcoholamine compound is one or more of diethanolisopropanolamine, diisopropanolamine and triisopropanolamine, and the mesh size range is 70-140 meshes.

7. The powder reinforcing agent for room temperature hardening according to claim 1, characterized in that: The borate compound is one or more of sodium tetraborate and potassium tetraborate, and the mesh size range is 80-150 mesh.

8. The method for preparing a powder reinforcing agent for room temperature hardening according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: Put microsilica fume, phosphate compound and cellulose modifier into a closed stirring kettle in sequence and stir evenly; S2: Add inorganic salt oxide powder and stir to mix evenly; S3: adding an amine compound and a borate compound, and continuing to stir to mix them evenly to obtain a powder reinforcing agent for room temperature curing.

9. The method for using the powder reinforcing agent for room temperature hardening according to any one of claims 1 to 7, characterized in that: According to the weight of the molding sand, the powder reinforcing agent is added in an amount of 1%-3% of the sand weight, the curing agent is added in an amount of 0.8%-2% of the sand weight, and they are mixed evenly with the molding sand in sequence. The inorganic binder is added in an amount of 2%-2.4% of the sand weight, and hardening can be achieved under normal temperature conditions.