Preparation method, product and application of lead-based chalcogenide core-shell structure quantum dot

By combining the thermal implantation method and the cation exchange method, the preparation process of lead-based chalcogen core-shell structure quantum dots is simplified, the problems of complex processes and environmental pollution in the existing technology are solved, and efficient and controllable quantum dot preparation and Self-assembled film generation enhances application potential.

CN118954443AInactive Publication Date: 2024-11-15CHANGCHUN UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411435115.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has complex process, environmental pollution, uneven particle size, uneven surface surface and low crystallinity problems in the preparation of lead-based chalcogen core-shell quantum dots, which limits its development in practical applications.

Method used

The combination of thermal injection method and cation exchange method is used to slowly evaporate the solvent to form a self-assembled film to prepare lead-based chalcogen core-shell structure quantum dots, which simplifies the process and improves the controllability and efficiency of the preparation.

Benefits of technology

The preparation of lead-based chalcogen core-shell structure quantum dots with low cost, high yield, multiple geometric structures can be prepared, mild reaction conditions, high repeatability and controllability is achieved, which simplifies the preparation process of self-assembled films and maintains the The structure and luminous intensity of quantum dots.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118954443A_ABST
    Figure CN118954443A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of semiconductor photoelectrons, in particular to a preparation method, a product and application of a lead-based chalcogenide core-shell structure quantum dot. The preparation method comprises the following steps: preparing lead-based chalcogenide quantum dots by using a thermal injection method; mixing cadmium oxide, oleic acid and 1-octadecene, and then carrying out stepped heating to obtain a cadmium oleate solution; the lead-based chalcogenide quantum dot solution is added into the cadmium oleate solution for a reaction, and the lead-based chalcogenide core-shell structure quantum dots are obtained; the lead-based chalcogenide quantum dots are PbSe quantum dots or PbS quantum dots. The lead-based chalcogenide quantum dots are prepared through a thermal injection method, the method has the advantages of being low in cost, high in yield and the like, and the size and shape of the quantum dots can be accurately regulated and controlled by controlling the reaction temperature and time. The lead-based chalcogenide core-shell structure quantum dots are prepared through a cation exchange method, and the method has the advantages that various geometric structures can be prepared, reaction conditions are mild, repeatability is high, controllability is high and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor optoelectronic technology, and in particular to a preparation method, product and application of lead-based chalcogenide core-shell structure quantum dots. Background Art

[0002] The study of semiconductor quantum dots occupies an important position in nanoscience. Colloidal quantum dots (CQDs) are synthesized by long-chain organic ligands (such as oleic acid, tri-n-octylphosphine), surface modified and aggregation-preventing methods to form a stable colloidal dispersion system in non-polar organic solvents. Monodispersed CQDs can be used as the basic components for bottom-up assembly of nanocrystalline superlattices. Through slow evaporation of solvents, the colloidal dispersion system of CQDs can generate self-assembled films, thereby realizing the scalable preparation of highly ordered quantum dot solids. This synergistic effect is of great significance for the material design of energy conversion, storage and nanoelectronic applications. These properties include enhanced charge transport capabilities, carrier delocalization, and unique optoelectronic properties. For example, self-assembled close-packed structures with oriented, exposed surfaces can improve the selectivity and activity of catalysts, thereby improving their overall performance and stability. In addition, well-organized mesoscopic structures also demonstrate optimized mass diffusion and adjustable micro-electric fields, thereby achieving higher performance in energy storage and electrocatalytic applications.

[0003] At present, the method for generating self-assembled films of colloidal quantum dots is mainly ligand exchange technology. Colloidal quantum dots are mainly synthesized by wet chemical methods. Organic ligands are used to control growth during the synthesis process, provide colloidal stability, and passivate dangling bonds on the surface. These organic ligands separate the quantum dots and form a barrier for electron transport. Since many applications require transmission, the original organic ligands are often replaced by shorter ligands. Since chemical reactions are used to replace existing ligands, the preparation process is more complicated and requires more steps and raw materials. It may also lead to unsatisfactory arrangement of quantum dots, affecting the structure and performance of quantum dots.

[0004] The quantum dots prepared by molecular beam epitaxy (MBE) and metal organic chemical vapor deposition (MOCVD) are limited by the substrate and the lattice constant of the quantum dots, which limits the types of quantum dots that can be prepared. In addition, these two methods are also inefficient in large-scale production because they cannot achieve high-speed and continuous preparation of quantum dots. Therefore, although these methods are of great significance in the research field, their shortcomings in practical applications also need to be seriously considered.

[0005] The process of preparing PbSe core-shell quantum dots by the alternating ion layer adsorption growth method (SILAR method) is complicated and has strict operating conditions, requiring the control of multiple factors such as temperature, pH value and reaction time. At the same time, this method is prone to produce a large amount of waste during the preparation process, causing certain pollution to the environment. In addition, the PbSe core-shell quantum dots prepared by the alternating ion layer adsorption method also have the disadvantages of uneven particle size, uneven surface and low crystallinity, which limits its further development and application in practical applications.

[0006] The ligand exchange technology for preparing self-assembled films requires replacing existing ligands through chemical reactions. The preparation process is more complicated and requires more steps and raw materials. It may also lead to unsatisfactory arrangement of quantum dots, affecting the structure and performance of quantum dots. Summary of the invention

[0007] Based on the above, the present invention provides a preparation method, product and application of self-assembled lead-based chalcogenide core-shell structure quantum dots. The present invention combines the hot injection method with the cation exchange method, and after the preparation of the lead-based chalcogenide core-shell structure quantum dots (such as PbSe), the colloidal dispersion system of the quantum dots can generate a self-assembled film by slowly evaporating the solvent.

[0008] To achieve the above object, the present invention provides the following solutions: One of the technical solutions of the present invention is a method for preparing lead-based chalcogenide core-shell structure quantum dots, comprising the following steps: Lead-based chalcogenide quantum dots were prepared by hot injection; The cadmium oxide, oleic acid and 1-octadecene are mixed and then heated in a stepwise manner to obtain a cadmium oleate solution; Adding the lead-based chalcogenide quantum dot solution to the cadmium oleate solution for reaction to obtain the lead-based chalcogenide core-shell structure quantum dots; The lead-based chalcogenide quantum dots are PbSe quantum dots or PbS quantum dots.

[0009] The second technical solution of the present invention is a lead-based chalcogenide core-shell structure quantum dot prepared according to the above-mentioned preparation method.

[0010] The third technical solution of the present invention is the use of the above-mentioned lead-based chalcogenide core-shell structure quantum dots in the preparation of self-assembled films.

[0011] A fourth technical solution of the present invention is a method for preparing a self-assembled film, comprising the following steps: dissolving the lead-based chalcogenide core-shell structure quantum dots in an organic solvent to obtain a mixed solution; The substrate is placed in the mixed solution, and the organic solvent is completely evaporated under vacuum drying conditions to obtain the self-assembled film.

[0012] A fifth technical solution of the present invention is a self-assembled film prepared according to the above-mentioned preparation method.

[0013] The sixth technical solution of the present invention is an energy storage or electrocatalytic material, the raw materials of which include the above-mentioned lead-based chalcogenide core-shell structure quantum dots or the above-mentioned self-assembled film.

[0014] The present invention discloses the following technical effects: The present invention prepares lead-based chalcogenide quantum dots by hot injection method, which has the advantages of low cost and high yield compared with molecular beam epitaxy (MBE) and metal organic chemical vapor deposition (MOCVD). By controlling the temperature and time of the reaction, the size and morphology of the quantum dots can be precisely controlled.

[0015] The present invention prepares lead-based chalcogenide core-shell structure quantum dots by a cation exchange method. Compared with the SILAR method, the cation exchange method has the characteristics of being able to prepare a variety of geometric structures, relatively mild reaction conditions, high repeatability and strong controllability.

[0016] Compared with traditional methods of generating self-assembled thin films, such as ligand exchange technology, the present invention generates self-assembled thin films by slow evaporation of solvents, which has a simpler and more economical preparation process. In this method, the solvent can be evaporated under mild conditions, so that the film is formed in a self-assembled manner without destroying the quantum dot structure and luminescence intensity. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 This is a photo of the quantum dot experimental environment of the present invention.

[0019] Figure 2 Schematic diagram of the preparation process of PbSe quantum dots of the present invention.

[0020] Figure 3 This is the PbSe quantum dot growth process in Example 1.

[0021] Figure 4 Schematic diagram of the preparation process of PbSe / CdSe quantum dots of the present invention.

[0022] Figure 5 This is the PbSe / CdSe quantum dot growth process in Example 1.

[0023] Figure 6 The following are photos of the self-assembled thin film generated by slow evaporation of the solvent in Example 1; wherein (a) is a photo of the Si substrate placed in a glass vial, and (b) is a photo of the vial sealed with a sealing film.

[0024] Figure 7 TEM images of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1; wherein (a), (b), and (c) are TEM images of PbSe quantum dots at different angles, and (d), (e), and (f) are TEM images of PbSe / CdSe quantum dots at different angles.

[0025] Figure 8 1 is the XRD spectrum of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1.

[0026] Fig. 9 1 and 2 are the absorption spectra of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1; wherein (a) is PbSe quantum dots and (b) is PbSe / CdSe quantum dots.

[0027] Fig.10 1 and 2 are the photoluminescence spectra of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1; wherein (a) is PbSe quantum dots and (b) is PbSe / CdSe quantum dots.

[0028] Fig.11 TEM images of PbS quantum dots and PbS / CdS quantum dots in Example 2; wherein (a) and (b) are TEM images of PbS quantum dots at different magnifications, and (c) and (d) are TEM images of PbS / CdS quantum dots at different angles.

[0029] Fig.12 2 is the XRD spectrum of PbS quantum dots and PbS / CdS quantum dots in Example 2.

[0030] Fig.13 2 are the photoluminescence spectra of PbS quantum dots and PbS / CdS quantum dots in Example 2.

[0031] Fig.14 TEM images of PbSe quantum dots and PbSe / CdSe quantum dots in Comparative Example 1; (a) PbSe quantum dots, (b) PbSe / CdSe quantum dots.

[0032] Fig.15 2 is the XRD spectrum of PbSe quantum dots and PbSe / CdSe quantum dots in Comparative Example 1.

[0033] Fig.16: The photoluminescence spectra of PbSe quantum dots and PbSe / CdSe quantum dots; (a) is PbSe quantum dots, and (b) is PbSe / CdSe quantum dots.

[0034] Fig.17 TEM images of PbSe quantum dots and PbSe / CdSe quantum dots prepared in Comparative Example 2; (a) is PbSe quantum dots, and (b) is PbSe / CdSe quantum dots. DETAILED DESCRIPTION

[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0036] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0037] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0038] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0039] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0040] One of the technical solutions of the present invention is a method for preparing lead-based chalcogenide core-shell structure quantum dots, comprising the following steps: Lead-based chalcogenide quantum dots were prepared by hot implantation; The cadmium oxide, oleic acid and 1-octadecene are mixed and then heated in a stepwise manner to obtain a cadmium oleate solution; Adding the lead-based chalcogenide quantum dot solution to the cadmium oleate solution for reaction to obtain the lead-based chalcogenide core-shell structure quantum dots; The lead-based chalcogenide quantum dots are PbSe quantum dots or PbS quantum dots.

[0041] In some embodiments of the present invention, the step heating is specifically as follows: first, the temperature is raised to 150°C at a rate of 4-6°C / min, then the temperature is continued to be raised to 180°C at a rate of 2-3°C / min and kept warm for 10 min, then the temperature is continued to be raised to 210°C at a rate of 2-3°C / min and kept warm for 10 min, and finally the temperature is continued to be raised to 240°C at a rate of 2-3°C / min and kept warm for 30~40 min.

[0042] In the present invention, the purpose of step heating is to obtain a solution with uniform temperature to prevent the quantum dots from aggregating and affecting the performance of the quantum dots.

[0043] If the temperature of each stage of gradient heating or the insulation time is adjusted beyond the parameter range recorded above, the temperature of the solution in the three-necked flask may be uneven, resulting in uneven quantum dot size or aggregation during the subsequent quantum dot growth process.

[0044] After the step heating, the method further comprises cooling the temperature to 100-120° C. at a rate of 3.5° C. / min.

[0045] In some embodiments of the present invention, the mass volume ratio of cadmium oxide, oleic acid and 1-octadecene is 1 g: 5-6 mL: 14-18 mL; When the lead-based chalcogenide quantum dot solution is added to the cadmium oleate solution for reaction, the temperature of the cadmium oleate solution is 100° C.; the reaction temperature is 100° C. and the reaction time is 30 min; the lead-based chalcogenide quantum dot solution is a n-hexane solution or a toluene solution of lead-based chalcogenide quantum dots; the Pb in the lead-based chalcogenide quantum dot solution is 2+ The Cd in the oleate cadmium solution 2+ The molar ratio is 1:36.

[0046] In some embodiments of the present invention, when the lead-based chalcogenide quantum dots are PbSe quantum dots, the preparation method thereof comprises the following steps: Dissolving Se powder in tri-n-octylphosphine to obtain a Se precursor; The lead source, oleic acid and 1-octadecene are mixed and then step-heated to obtain a mixed solution; Adding the Se precursor to the mixed solution and reacting at 140-170° C. for 1-25 min to obtain the PbSe quantum dots; the molar ratio of the Se powder to the lead source is 3-5:1; The lead source is lead oxide and / or lead acetate.

[0047] After the reaction is completed, the steps of cooling the product to room temperature in an ice-water bath and removing excess substances in the product by centrifugation are also included.

[0048] The purpose of step heating in this step is to gradually dissolve PbO and ensure that the temperature of the solution in the three-necked flask is uniform.

[0049] In some embodiments of the present invention, when the lead-based chalcogenide quantum dots are PbS quantum dots, the preparation method thereof comprises the following steps: A lead source, oleic acid and 1-octadecene are mixed and then step-heated to obtain a lead oleate precursor; Adding 1-octadecene and hexamethyldisilathione (TMS) 2S to the lead oleate precursor and reacting at 90°C for 1-25min to obtain PbS quantum dots; when adding 1-octadecene and (TMS) 2S to the lead oleate precursor, the temperature of the lead oleate precursor is 90°C; The mass volume ratio of the lead source to the (TMS)2S is 400-500 mg:210 μL; The lead source is lead oxide and / or lead acetate.

[0050] The present invention can regulate the size and shape of quantum dots by controlling the growth temperature or growth time of quantum dots.

[0051] The second technical solution of the present invention is a lead-based chalcogenide core-shell structure quantum dot prepared according to the above-mentioned preparation method.

[0052] The third technical solution of the present invention is the use of the above-mentioned lead-based chalcogenide core-shell structure quantum dots in the preparation of self-assembled films.

[0053] A fourth technical solution of the present invention is a method for preparing a self-assembled film, comprising the following steps: dissolving the lead-based chalcogenide core-shell structure quantum dots in an organic solvent to obtain a mixed solution; The substrate is placed in the mixed solution, and the organic solvent is completely evaporated under vacuum drying conditions to obtain the self-assembled film. The organic solvent is n-hexane or toluene.

[0054] A fifth technical solution of the present invention is a self-assembled film prepared according to the above-mentioned preparation method.

[0055] The sixth technical solution of the present invention is an energy storage or electrocatalytic material, the raw materials of which include the above-mentioned lead-based chalcogenide core-shell structure quantum dots or the above-mentioned self-assembled film.

[0056] The technical solutions described in the present invention, unless otherwise specified, are all conventional solutions in the art, and the reagents or raw materials used, unless otherwise specified, are purchased from commercial channels or have been disclosed.

[0057] The quantum dot experimental device of the present invention is built in a fume hood. Two constant temperature heating magnetic stirrers are placed at the bottom. A three-necked bottle is placed in the magnetic stirrer and fixed with an iron clamp. A condenser is connected to the upper end of the three-necked bottle to prevent the solvent from volatilizing and losing during the heating process, so that it condenses and refluxes. Figure 1 As shown. The upper end of the condenser is connected to a gas exchange device. The left side of the figure shows a double row of pipes connected to high-purity nitrogen and a vacuum pump respectively. The exhaust port on the right side of the double row of pipes is connected to a glycerol indicator. The entire system constitutes a Schlenk double row vacuum system for synthesizing colloidal quantum dots by hot injection and cation exchange methods, which meets the anhydrous and oxygen-free environment required for synthesizing colloidal quantum dots.

[0058] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0059] The schematic diagram of the preparation process of PbSe quantum dots of the present invention is as follows Figure 2 The schematic diagram of the preparation process of PbSe / CdSe quantum dots of the present invention is shown in Figure 4 shown.

[0060] Example 1 Step 1: Preparation of PbSe quantum dots by hot injection Preparation of Se precursor: Add 12.8 mL of tri-n-octylphosphine (TOP) to a 50 mL beaker, weigh 1.28 g of Se powder and pour it into the 50 mL beaker containing TOP solution, put it into a magnetic rotor, seal it with a sealing film, and stir for more than 2 h to allow the Se powder to fully dissolve in the TOP solution, until the Se powder is completely dissolved to obtain a transparent and clear solution, that is, the preparation of Se precursor is completed; 0.892 g of lead oxide (PbO), 6.3 mL of oleic acid (OA) and 32.56 mL of 1-octadecene (ODE) solution were added to a three-necked flask, and a magnetic rotor was placed to stir at 25 °C. After the pipeline was connected, the vacuum pump was turned on to extract the air in the solution. This process lasted for 25 min. After the nitrogen was passed for 15 min, the reaction was carried out in a nitrogen environment. After the nitrogen was passed, the solution was heated stepwise to 50 °C, then to 110 °C, and finally to the required reaction temperature of 160 °C. This temperature was maintained for 1 h to obtain a liquid with uniform temperature. During this process, PbO will gradually dissolve and the solution will become a light yellow clear liquid. After that, the Se precursor was injected into the three-necked flask and reacted for 150 s. After the reaction was completed, an ice water bath was immediately placed. When the solution temperature drops to room temperature, extract the product after the reaction into a centrifuge tube, add hexane: acetone: ethanol = 2:2:1, then mix the centrifuge tube evenly and put it into a centrifuge, centrifuge at 7000 rpm for 5 min, repeat the above centrifugation steps 3 times, this process can remove excess substances in the product. Use a balance to weigh the quantum dots and dissolve them in hexane and toluene respectively to obtain PbSe quantum dot hexane solution and PbSe quantum dot toluene solution, which are sealed and stored in a dark environment at 4 °C. The growth process of PbSe quantum dots in this step is as follows Figure 3 shown.

[0061] Step 2: Preparation of PbSe / CdSe quantum dots by cation exchange method First, add a magnetic rotor, 1.5 g cadmium oxide (CdO), 9 mL oleic acid (OA) and 22 mL 1-octadecene (ODE) to a three-necked flask. Vacuum without stirring for 10 min, then restore nitrogen, adjust the magnetic rotor to a medium speed, heat to 150 °C, and at 110 °C, the solution will splash and the solution will be bright red. Continue to increase the temperature to 180 °C, and the solution will be dark red. Adjust the magnetic rotor to the maximum speed and maintain this temperature for 10 min. Increase the temperature to 210 °C, maintain this temperature for 10 min, and increase the temperature to 240 °C. The solution is now yellow and turbid. After maintaining this temperature for 40 min, the solution is light yellow and clear. At this time, cool it to 100 °C, extract the air in the solution, and maintain this process for 20 min. Restore the nitrogen environment and maintain it for 10 min. At this time, quickly inject 10 mL of 6 mg / mL PbSe quantum dot toluene solution into the oleic acid cadmium solution. After reacting for 30 min, use an ice water bath to cool it to room temperature. The synthesized PbSe / CdSe quantum dot crude solution was transferred to a centrifuge tube and mixed with ethanol at a volume ratio of 1:1 to precipitate the quantum dots. Then, the solution was centrifuged at 7000 rpm for 10 min to obtain quantum dot powder. After dissolving with toluene solution, ethanol solution was added to precipitate the quantum dots, and then centrifuged again. This washing process was repeated three times. Finally, the obtained quantum dots were dispersed in n-hexane and toluene, respectively, to obtain PbSe / CdSe quantum dot n-hexane solution and PbSe / CdSe quantum dot toluene solution, which were sealed and stored in a dark environment at 4 °C. The growth process of PbSe / CdSe quantum dots in this step is as follows: Figure 5 shown.

[0062] Step 3: Generating a self-assembled film by slow evaporation of the solvent First, the Si substrate was cut into 1×1 cm 2Size, the cut Si substrate was ultrasonically cleaned in isopropanol, acetone, ethanol and deionized water for 15 min each, and dried with a nitrogen gun. The cleaned Si substrate was placed face up in a plasma machine for plasma cleaning for 15 min. After the plasma machine treatment was completed, a drop of deionized water was dropped on the Si substrate. When the water could be spread on the entire substrate, the Si substrate treatment was completed. A solution of (3-mercaptopropyl)trimethoxysilane (MPTS) and n-hexane in a ratio of 4:1 was prepared, and the Si substrate was immersed in the solution for 12 h (the function of this solution was to modify the surface of the Si substrate. The purpose of immersion was to form a sulfide modification layer, improve the adhesion of the Si substrate, and enhance its dispersibility and stability). Before the self-assembly experiment, the substrate was rinsed with n-hexane and dried with a nitrogen gun. The Si substrate was then placed in a clean 5 mL glass vial to allow the Si substrate to be further placed at a 45° angle (face up for self-assembly). Pour 3 mL of the prepared PbSe quantum dots and PbSe / CdSe quantum dots (concentration of 10 mg / mL, n-hexane solution) into small vials, respectively, and seal them with a sealing film with three small holes for solvent evaporation (such as Figure 6 Finally, the self-assembled sample in the vial was dried in a vacuum desiccator at 25 °C for 24 h to ensure complete evaporation of the solvent.

[0063] First, 10 mL of PbSe quantum dots and PbSe / CdSe quantum dots (concentration of 1 mg / mL, n-hexane solution) were ultrasonically poured into centrifuge tubes respectively, and the copper mesh covered with carbon film was immersed in the centrifuge tube for 30 seconds, and then the copper mesh was immersed in the methanol solution again for 30 seconds. The process (i.e., the steps of immersing in the centrifuge tube and immersing in the methanol solution) was repeated three times. Finally, the copper mesh was dried in a vacuum desiccator at 25°C for 1 h to ensure complete evaporation of the solvent.

[0064] Finally, the copper mesh and Si substrate were tested by TEM, XRD, absorption spectrum and photoluminescence spectrum.

[0065] Figure 7 TEM images of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1; (a), (b), and (c) are PbSe quantum dots, and (c), (d), and (e) are PbSe / CdSe quantum dots. Figure 7 It can be seen that the size of the quantum dots is relatively uniform, and this self-assembly technology provides perfect cubic order close to the superlattice, which is different from the monodispersity of traditional quantum dots.

[0066] Figure 8 The XRD patterns of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1 are shown in FIG. Figure 8It can be seen that it matches the standard PDF card, proving that the synthesized quantum dots are PbSe and PbSe / CdSe structures, and no other impurity peaks are introduced.

[0067] Fig. 9 The absorption spectra of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1 are shown in Figure 1; (a) is PbSe quantum dots, and (b) is PbSe / CdSe quantum dots. Fig. 9 It can be seen that the absorption peak of the PbSe / CdSe quantum dots generated by cation exchange is blue-shifted compared with the PbSe quantum dots.

[0068] Fig.10 The photoluminescence spectra of PbSe quantum dots and PbSe / CdSe quantum dots in Example 1 are shown in Figure 2; (a) is PbSe quantum dots and (b) is PbSe / CdSe quantum dots. Fig.10 It can be seen that the formation of self-assembled films by slow evaporation of the solvent does not lead to a decrease in the luminescence intensity, and the FWHM of the prepared quantum dots is narrow, indicating that the quality of the synthesis is good.

[0069] Example 2 Step 1: Preparation of PbS quantum dots by hot injection Preparation of lead oleate precursor: 446 mg PbO, 1.5 mL OA, 20 mL ODE and a magnetic stirring rotor were placed in a 100 mL three-necked flask. The thermometer of the heating magnetic stirring table was kept below the liquid level so that the thermometer and the magnetic rotor would not contact each other as much as possible, otherwise the accuracy of the temperature measurement would be affected. The three-necked flask was connected to the Schrank system, and the air in the flask was removed by vacuuming and passing nitrogen three times. While keeping the nitrogen flowing, the mixture was first heated to 50 °C at 5 °C / min and kept for 10 min, then heated to 100 °C at 5 °C / min, and stirred vigorously at this temperature for 1 h, and then further increased to 120 °C at 3 °C / min, and the nitrogen was stopped. After vacuuming for 30 min, the transparent and clear lead oleate precursor was prepared.

[0070] Continue to maintain the nitrogen environment, cool the cadmium oleate solution to 90 °C, and immediately inject a mixed solution of 5 mL ODE and 210 μL hexamethyldisilathione (TMS) 2S with a long syringe after the temperature stabilizes. At this time, the solution immediately turns brown and then black. After reacting at 90 °C for 90 s, immediately inject excess n-hexane to extinguish the reaction, and cool the solution to room temperature with an ice water bath to obtain a crude PbS quantum dot solution.

[0071] Use a dropper to put the obtained PbS quantum dot crude solution into multiple 10 mL centrifuge tubes, and add the PbS quantum dot crude solution: acetone: ethanol volume ratio = 2:2:1 acetone ethanol solution to the centrifuge tube to fully precipitate the quantum dots. Put the quantum dots into a centrifuge and centrifuge at 5000 rpm for five minutes. Pour the supernatant. The PbS quantum dots are attached to the wall of the centrifuge tube. Continue to add n-hexane solution to dissolve the PbS quantum dots. Repeat the above centrifugation-dissolving quantum dot process three times, use a balance to weigh the quantum dots and dissolve them in n-hexane and toluene respectively, and seal and store them in a dark environment at 4 °C.

[0072] Step 2: Preparation of PbS / CdS quantum dots by cation exchange method Preparation of cadmium oleate solution: 0.582 g CdO, 3 mL OA, 10 mL ODE and a clean magnetic stirring rotor were placed in a three-necked flask, and the three-necked flask was connected to a Schrank double-row system. After the air in the three-necked flask was removed by continuous vacuuming and nitrogen gas flow, the magnetic stirring rotor was adjusted to a suitable speed, and the solution was step-heated to 240 ° C (the temperature and time of step heating were the same as the step heating process in step 2 of Example 1), and maintained at this temperature for 30 min to form a transparent and clear solution. The solution was then cooled to 120 ° C under a nitrogen flow, vacuumed for 30 min, and then further cooled to 100 ° C as the reaction temperature for cation exchange.

[0073] Formation of PbS / CdS quantum dots: After the temperature of the cadmium oleate solution stabilized at 100 °C, the PbS quantum dot toluene solution was injected into the three-necked flask. 2+ with cd 2+ The ratio of the molar concentration of the substance is 1:36. The speed of the magnetic stirrer was increased to react for 30 minutes to form a CdS shell. The obtained crude solution of PbS / CdS quantum dots was added to an equal volume of ethanol solution to fully precipitate the quantum dots. The PbS / CdS solution was centrifuged at a speed of 7000 rpm to separate the PbS / CdS quantum dots from the organic solvent. The clarified solution was poured out, and the quantum dots attached to the wall of the test tube were dispersed with toluene solution, and the quantum dots were precipitated and centrifuged. The cleaning process (dispersion with toluene solution-precipitation centrifugation step) was repeated three times, and the quantum dots were weighed using a balance and dissolved in n-hexane and toluene, and sealed and stored in a dark environment at 4 °C.

[0074] Step 3: Generating a self-assembled film by slow evaporation of the solvent First, the Si substrate was cut into 1×1 cm 2Size, the cut Si substrate was ultrasonically cleaned in isopropanol, acetone, ethanol and deionized water for 15 min each, and dried with a nitrogen gun. The cleaned Si substrate was placed face up in a plasma machine for plasma cleaning for 15 min. After the plasma machine treatment was completed, a drop of deionized water was dropped on the Si substrate. When the water could be spread on the entire substrate, the Si substrate treatment was completed. A solution of (3-mercaptopropyl)trimethoxysilane (MPTS) and n-hexane in a ratio of 4:1 was prepared, and the Si substrate was immersed in the solution for 12 h. Before the self-assembly experiment, the substrate was rinsed with n-hexane and dried with a nitrogen gun. The Si substrate was then placed in a clean 5 mL glass vial to allow the Si substrate to be further placed at a 45 ° angle (face up for self-assembly). 3 mL of the prepared PbS quantum dots and PbS / CdS quantum dots (concentration of 10 mg / mL, n-hexane solution) were poured into the vials respectively and sealed with a sealing film with three small holes for solvent evaporation. Finally, the self-assembled samples in the vials were dried in a vacuum desiccator at 25 °C for 24 h to ensure complete evaporation of the solvent.

[0075] First, 10 mL of PbS quantum dots and PbS / CdS quantum dots (concentration of 1 mg / mL, n-hexane solution) were ultrasonically poured into centrifuge tubes respectively, and the copper mesh covered with carbon film was immersed in the centrifuge tube for 30 seconds, and then the copper mesh was immersed in the methanol solution again for 30 seconds. The process (i.e., the steps of immersing in the centrifuge tube and immersing in the methanol solution) was repeated three times. Finally, the copper mesh was dried in a vacuum desiccator at 25°C for 1 h to ensure complete evaporation of the solvent.

[0076] Finally, the copper mesh and Si substrate were tested by TEM, XRD and photoluminescence spectrum.

[0077] Fig.11 TEM images of PbS quantum dots and PbS / CdS quantum dots in Example 2; (a) and (b) are PbS quantum dots, and (c) and (d) are PbS / CdS quantum dots. Fig.11 It can be seen that the quantum dots exhibit a spherical structure and uniform size, indicating excellent monodispersity.

[0078] Fig.12 The XRD patterns of PbS quantum dots and PbS / CdS quantum dots in Example 2 are shown in FIG. Fig.12 It can be seen that the diffraction peaks are consistent with those of the PDF standard card, indicating the high purity and high crystallinity of PbS quantum dots and PbS / CdS.

[0079] Fig.13 is the photoluminescence spectrum of PbS quantum dots and PbS / CdS quantum dots in Example 2. Fig.13It can be seen that the emission peak of quantum dots after cation exchange is blue-shifted, and the band edge emission of quantum dots at the low energy end is improved to a certain extent, indicating that the introduction of CdS shell can passivate the defects on the surface of PbS quantum dots.

[0080] Comparative Example 1 Step 1 is the same as step 1 in Example 1.

[0081] Step 2 is the same as step 2 of Example 1.

[0082] Step 3, first ultrasonically clean the Si substrate in isopropanol, acetone, ethanol and deionized water for 15 minutes each, and blow dry with a nitrogen gun. Place the cleaned Si substrate face up in the plasma machine for plasma cleaning for 15 minutes. After the plasma machine treatment is completed, drop a drop of deionized water on the Si substrate. When the water can be spread on the entire substrate, the Si substrate treatment is completed. Drop 3 mL of PbSe quantum dots and PbSe / CdSe quantum dots (concentration of 10 mg / mL, n-hexane solution) prepared above on the Si substrate respectively, and finally put the dropped Si substrate into a vacuum dryer to completely evaporate it.

[0083] 10 mL of PbSe quantum dots and PbSe / CdSe quantum dots (concentration of 1 mg / mL, n-hexane solution) were dropped onto the copper grid covered with carbon film, and the copper grid was placed in a vacuum desiccator for more than 1 h to ensure complete evaporation of the solvent.

[0084] Finally, the copper mesh and Si substrate were tested by TEM, XRD and photoluminescence spectrum.

[0085] Fig.14 TEM images of PbSe quantum dots and PbSe / CdSe quantum dots in Comparative Example 1; (a) is PbSe quantum dots, and (b) is PbSe / CdSe quantum dots. Fig.14 It can be seen that the size of the quantum dots is relatively uniform and has good monodispersity, but there is no self-assembly phenomenon.

[0086] Fig.15 The XRD patterns of PbSe quantum dots and PbSe / CdSe quantum dots in Comparative Example 1 are shown in FIG. Fig.15 It can be seen that the diffraction peak is consistent with the PDF standard card, but the quality of the film on the surface of the Si substrate is poor, resulting in a stronger diffraction peak of the Si substrate and poor quality of the measured XRD pattern.

[0087] Fig.16 The photoluminescence spectra of PbSe quantum dots and PbSe / CdSe quantum dots are shown in Figure 2. (a) is PbSe quantum dots and (b) is PbSe / CdSe quantum dots. Fig.16It can be seen that the luminescence intensity is low at room temperature, indicating that the film quality on the surface of the Si substrate is poor.

[0088] Comparative Example 2 Step 1: Preparation of PbSe quantum dots by hot injection Preparation of Se precursor: Add 12.8 mL of tri-n-octylphosphine (TOP) to a 50 mL beaker, weigh 1.28 g of Se powder and pour it into the 50 mL beaker containing TOP solution, put it into a magnetic rotor, seal it with a sealing film, and stir for more than 2 h to allow the Se powder to fully dissolve in the TOP solution, until the Se powder is completely dissolved to obtain a transparent and clear solution, that is, the preparation of Se precursor is completed; Add 0.892 g of lead oxide (PbO), 6.3 mL of oleic acid (OA) and 32.56 mL of 1-octadecene (ODE) solution to a three-necked flask, and place in a magnetic rotor to stir at 25 °C. After the pipeline is connected, turn on the vacuum pump to extract the air in the solution. This process lasts for 25 min. After the end, nitrogen is passed for 15 min to allow the reaction to proceed in a nitrogen environment. The temperature is directly raised to the reaction temperature of 160 °C without step heating, and this temperature is maintained for 1 h to obtain a liquid with uniform temperature. During this process, PbO will gradually dissolve and the solution will become a light yellow clear liquid. After that, the Se precursor is injected into the three-necked flask, reacted for 150 s, and immediately placed in an ice water bath after the reaction is completed. When the solution temperature drops to room temperature, extract the product after the reaction into a centrifuge tube, add n-hexane: acetone: ethanol = 2:2:1, then mix the centrifuge tube evenly and put it into a centrifuge, centrifuge at 7000 rpm for 5 minutes, repeat the above centrifugation steps 3 times, this process can remove the excess substances in the product. Weigh the quantum dots using a balance and dissolve them in n-hexane and toluene respectively, and store them in a sealed and dark environment at 4 °C.

[0089] Step 2 is the same as step 2 of Example 1.

[0090] In step 3, 10 mL of PbSe quantum dots and PbSe / CdSe quantum dots (concentration of 1 mg / mL, n-hexane solution) were first ultrasonically poured into centrifuge tubes respectively, the copper mesh covered with carbon film was immersed in the centrifuge tube for 30 seconds, and then the copper mesh was immersed in the methanol solution again for 30 seconds. This process (i.e., the steps of immersing in the centrifuge tube and immersing in the methanol solution) was repeated three times. Finally, the copper mesh was dried in a vacuum dryer at 25 °C for 1 h to ensure complete evaporation of the solvent.

[0091] Finally, the copper mesh was subjected to TEM test.

[0092] Fig.17TEM images of PbSe quantum dots and PbSe / CdSe quantum dots prepared in Comparative Example 2; (a) is PbSe quantum dots, and (b) is PbSe / CdSe quantum dots. Fig.17 It can be seen that the quantum dots are aggregated, the sizes are uneven, and the quantum dots are not monodisperse.

[0093] From the TEM data of Example 1 above, it can be seen that the size of the quantum dots prepared by the method of the present invention is relatively uniform, and this self-assembly technology provides perfect cubic order close to the superlattice, which is different from the monodispersity of traditional quantum dots. The quantum dot self-assembled film prepared by the present invention is characterized by XRD, and it is found through analysis that it matches the standard PDF card, proving that the synthesized QDs are PbSe structures and no other impurity peaks are introduced. From the absorption spectrum and photoluminescence spectrum, it can be seen that the self-assembled film generated by slow evaporation of the solvent does not lead to a decrease in luminescence intensity, and the FWHM of the prepared quantum dots is narrow, indicating that the quality of the synthesis is good.

[0094] From the comparative TEM results, we can see that without using the slow evaporation of solvent, the quantum dots still maintain monodispersity, but no self-assembly phenomenon occurs. Not using step heating in the preparation of quantum dots will cause quantum dots to aggregate, and no luminescence peak appears in the photoluminescence test.

[0095] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing lead-based chalcogenide core-shell structure quantum dots, It is characterized in that The following steps are involved: Lead-based chalcogenide quantum dots were prepared by hot implantation; The cadmium oxide, oleic acid and 1-octadecene are mixed and then heated in a stepwise manner to obtain a cadmium oleate solution; Adding the lead-based chalcogenide quantum dot solution to the cadmium oleate solution for reaction to obtain the lead-based chalcogenide core-shell structure quantum dots; The lead-based chalcogenide quantum dots are PbSe quantum dots or PbS quantum dots; The step heating is specifically as follows: first, the temperature is raised to 150°C at a rate of 4-6°C / min, then the temperature is continued to be raised to 180°C at a rate of 2-3°C / min and kept warm for 10 min, then the temperature is continued to be raised to 210°C at a rate of 2-3°C / min and kept warm for 10 min, and finally the temperature is continued to be raised to 240°C at a rate of 2-3°C / min and kept warm for 30-40 min.

2. The method for preparing lead-based chalcogenide core-shell structure quantum dots according to claim 1, It is characterized in that The mass volume ratio of the cadmium oxide, oleic acid and 1-octadecene is 1 g: 5-6 mL: 14-18 mL; When the lead-based chalcogenide quantum dot solution is added to the cadmium oleate solution for reaction, the temperature of the cadmium oleate solution is 100° C.; the reaction temperature is 100° C., and the reaction time is 30-90 min; the lead-based chalcogenide quantum dot solution is a n-hexane solution or a toluene solution of lead-based chalcogenide quantum dots; Pb in the lead-based chalcogenide quantum dot solution 2+ The Cd in the oleate cadmium solution 2+ The molar ratio is 1:

36.

3. The method for preparing lead-based chalcogenide core-shell structure quantum dots according to claim 1, It is characterized in that When the lead-based chalcogenide quantum dots are PbSe quantum dots, the preparation method thereof comprises the following steps: Dissolving Se powder in tri-n-octylphosphine to obtain a Se precursor; The lead source, oleic acid and 1-octadecene are mixed and then step-heated to obtain a mixed solution; Adding the Se precursor to the mixed solution and reacting at 140-170° C. for 1-25 min to obtain the PbSe quantum dots; the molar ratio of the Se powder to the lead source is 3-5:1; The lead source is lead oxide and / or lead acetate.

4. The method for preparing lead-based chalcogenide core-shell structure quantum dots according to claim 1, It is characterized in that When the lead-based chalcogenide quantum dots are PbS quantum dots, the preparation method thereof comprises the following steps: A lead source, oleic acid and 1-octadecene are mixed and then step-heated to obtain a lead oleate precursor; Adding 1-octadecene and hexamethyldisilathione to the lead oleate precursor and reacting at 90° C. for 1-25 minutes to obtain PbS quantum dots; The mass volume ratio of the lead source to the (TMS)2S is 400-500 mg:210 μL; The lead source is lead oxide and / or lead acetate.

5. Lead-based chalcogenide core-shell structure quantum dots prepared according to the preparation method according to any one of claims 1 to 4.

6. Use of the lead-based chalcogenide core-shell structure quantum dots as claimed in claim 5 in the preparation of self-assembled films.

7. A method for preparing a self-assembled film, It is characterized in that The method comprises the following steps: dissolving the lead-based chalcogenide core-shell structure quantum dots according to claim 6 in an organic solvent to obtain a mixed solution; The substrate is placed in the mixed solution, and the organic solvent is completely evaporated under vacuum drying conditions to obtain the self-assembled film.

8. The self-assembled film prepared by the preparation method according to claim 7.

9. An energy storage or electrocatalytic material, It is characterized in that The raw materials include the lead-based chalcogenide core-shell structure quantum dots described in claim 6 or the self-assembled film described in claim 8.

Citation Information

Patent Citations

  • Cadmium-free quantum dot and preparation method thereof

    CN111303882A

  • Quantum dot pixelated film and preparation method thereof

    CN113651286A

  • Method for synthesizing CdSe quantum dots at gradient variable temperature and CdSe quantum dots

    CN114479862A

  • Lead group core-shell structure quantum dot and preparation method thereof

    CN116814244A