Preparation process and preparation device of low-alkali low-viscosity magnesium silicate and working method of preparation device
By using aluminum silicate solution as a silicon source and pH regulator and controlling the reaction conditions, low alkalinity and low viscosity magnesium silicate were successfully prepared, solving the problems of high production process cost and high energy consumption in the prior art. A low-cost and efficient preparation of magnesium silicate is achieved.
Patent Information
- Application Number
- CN202411011842.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The prior art is difficult to effectively design a low-alkaline and low-viscosity magnesium silicate preparation process, and there are problems of high cost and high energy consumption.
Aluminum silicate solution is used as the silicon source and pH regulator. By gradually adding magnesium oxide solution and controlling the reaction pH value is within the range of 8.5-10, magnesium silicate is generated, and a viscosity reducing agent is added after the reaction is completed to ensure aluminum silicate. In excess, filtration and recycling are subsequently performed.
The preparation of low-alkaline magnesium silicate is achieved, which reduces raw material costs and production process complexity, simplifies supply chain management, improves thermal energy utilization and equipment efficiency, and achieves cost reduction through recycling of raw materials and nitrogen.
Smart Images

Figure CN118954524A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium silicate preparation, and in particular to a low-alkali and low-viscosity magnesium silicate preparation process, a preparation device and a working method of the device. Background Art
[0002] Magnesium silicate is an important industrial raw material, especially in the manufacture of coatings, adhesives and high-performance polymers. Magnesium silicate with different properties has different application scenarios; among them, low alkalinity and low viscosity are key performance indicators of magnesium silicate, which can improve the stability and handling performance of the product.
[0003] Regarding the preparation of low-alkalinity, low-viscosity magnesium silicate, the inventors believe that how to design a preparation process for low-alkalinity, low-viscosity magnesium silicate and ensure that the preparation process has the advantages of low cost and low energy consumption is a technical problem that general technicians in this field need to solve.
[0004] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0005] In view of the above technical problems, the embodiments of the present invention provide a low-alkali and low-viscosity magnesium silicate preparation process, a preparation device and a working method of the device to solve the problems raised in the above background technology.
[0006] The present invention provides the following technical solutions:
[0007] A low-alkali and low-viscosity magnesium silicate preparation process, comprising:
[0008] S1, respectively preparing aluminum silicate solution and magnesium oxide solution;
[0009] Among them, aluminum silicate solution is used as silicon source and pH regulator in the reaction, and magnesium oxide solution is used as magnesium source in the reaction;
[0010] S2, gradually adding the magnesium oxide solution to the aluminum silicate solution, so that the magnesium oxide solution reacts with the aluminum silicate solution to generate magnesium silicate;
[0011] S3. During the reaction, according to the pH value of the reaction solution, the aluminum silicate solution is gradually added to the reaction solution to maintain the reaction pH value range; the pH value range is controlled between 8.5-10;
[0012] S4. After the reaction is completed, continue to add aluminum silicate solution to the reaction solution to ensure that aluminum silicate is in excess in the reaction solution at the end of the reaction; at the same time, add a viscosity reducer to the reaction solution;
[0013] S5. After the aluminum silicate in the reaction solution is in an excess state, the reaction solution is filtered and the reaction filtrate is recovered; at the same time, the magnesium silicate removed from the reaction solution is recovered.
[0014] A preparation device for low-alkali and low-viscosity magnesium silicate; comprising:
[0015] Reactor, aluminum silicate tank, nitrogen storage tank and nitrogen temporary storage tank;
[0016] The first discharge port of the aluminum silicate tank is connected to the aluminum silicate inlet of the reactor through a pipeline; the first feed valve is connected in series to the pipeline connecting the first discharge port of the aluminum silicate tank and the aluminum silicate inlet of the reactor;
[0017] A heating coil is arranged around the outer wall of the reactor, and the cross section of the heating coil is rectangular; the hot water inlet of the heating coil is located at one side of the bottom of the reactor, and the hot water outlet of the heating coil is located at one side of the top of the reactor;
[0018] An insulating coil is arranged around the outside of the heating coil; the cross section of the insulating coil is rectangular, and the pipe walls of adjacent insulating coils are arranged close to the wall;
[0019] The second discharge port of the aluminum silicate tank and the first nitrogen outlet of the nitrogen storage tank are respectively connected to the upper straight port and the lower straight port of the first three-way pipe, and the branch port of the first three-way pipe is connected to the inlet of the insulation coil;
[0020] A second feed valve and a pump body are connected in series to the pipeline connecting the second discharge port of the aluminum silicate tank and the upper straight port of the first three-way pipe; a first air inlet valve is connected in series to the pipeline connecting the first nitrogen outlet of the nitrogen storage tank and the lower straight port of the first three-way pipe;
[0021] The first nitrogen inlet of the nitrogen temporary storage tank and the outlet of the heat-insulating coil are respectively connected to the upper straight port and the lower straight port of the second three-way pipe; the branch port of the second three-way pipe is connected to the spray pipe arranged in the reactor through a pipeline;
[0022] The second air inlet valve, the first air pump, and the gas flow meter are connected in series to the pipeline connecting the first nitrogen inlet of the nitrogen temporary storage tank and the upper straight port of the second three-way pipe; the first liquid outlet valve is connected in series to the pipeline connecting the branch port of the second three-way pipe and the spray pipe;
[0023] The second nitrogen outlet of the nitrogen temporary storage tank is connected to the second nitrogen inlet of the nitrogen storage tank through a pipeline, and the pipeline connecting the second nitrogen outlet of the nitrogen temporary storage tank and the second nitrogen inlet of the nitrogen storage tank is connected in series with an outlet valve and a second air pump;
[0024] The discharge port at the bottom of the reactor is connected to the upper straight port of the third three-way pipe, the lower straight port of the third three-way pipe is connected to the discharge valve, and the branch port of the third three-way pipe is connected to the liquid inlet of the aluminum silicate tank through a pipeline; the pipeline connecting the branch port of the third three-way pipe and the liquid inlet of the aluminum silicate tank is connected in series with a filter valve, a circulation pump body, and a liquid return valve;
[0025] Wherein, a liquid adding port and an exhaust valve are arranged on the top of the reactor.
[0026] Preferably, a filter is connected in series to the pipeline connecting the branch of the third three-way pipe and the liquid inlet of the aluminum silicate tank; an agitator, a thermometer, and a pH sensor are provided inside the reactor; and a sight glass is connected in series to the pipeline connected in series to the first liquid outlet valve.
[0027] Preferably, a heat-insulating jacket is provided on the outside of the heat-insulating coil on the reactor, and the heat-insulating jacket is filled with heat-insulating material.
[0028] Preferably, the stirrer comprises a main stirring shaft, an upper stirring blade, a lower stirring blade, a scraper, a synchronous gear, a driving gear, an auxiliary stirring shaft, and a stirring blade;
[0029] The stirring shaft is located in the reactor and is vertically rotatably connected to the reactor;
[0030] The upper stirring blade and the lower stirring blade are arranged at intervals in the upper and lower parts, the upper stirring blade is fixed on the upper half of the stirring shaft, and the lower stirring blade is fixed on the lower half of the stirring shaft;
[0031] The scrapers include two, and the two scrapers are respectively fixedly connected to the ends of the upper stirring blade and the lower stirring blade on the same side;
[0032] The synchronous gear is fixed on the main stirring shaft, and the synchronous gear is located above the upper stirring blade;
[0033] The auxiliary stirring shafts include two, which are located on both sides of the stirring shaft, and the upper and lower ends of the auxiliary stirring shafts are rotatably connected to the upper stirring blade and the lower stirring blade respectively, and the upper ends of the auxiliary stirring shafts protrude upward outside the upper stirring blade;
[0034] The driving gears include two, which are respectively fixed on the upper ends of the auxiliary stirring shafts; the two driving gears are respectively meshed with synchronous gears for transmission; and each auxiliary stirring shaft is provided with a plurality of stirring blades.
[0035] A working method of the low-alkali and low-viscosity magnesium silicate preparation device as described above comprises the following steps:
[0036] S61, respectively preparing an aluminum silicate solution and a magnesium oxide solution, wherein the aluminum silicate solution is stored in an aluminum silicate tank; the magnesium oxide solution is stored in a temporary storage tank; opening a first feed valve, and conveying a certain amount of aluminum silicate solution from the aluminum silicate tank to the reactor as a silicon source and a pH adjuster in the reaction; and then closing the first feed valve;
[0037] S62, adding the magnesium oxide solution in the temporary storage tank into the reactor through the liquid adding port on the reactor to react; and introducing hot water from the hot water inlet of the heating coil to heat the materials in the reactor;
[0038] S63, during the reaction process, close the first liquid outlet valve; open the first air inlet valve, the second air inlet valve, and the first air pump in sequence, and the nitrogen in the nitrogen storage tank enters the insulation coil along the inlet of the insulation coil. When the gas flow rate detected by the gas flow meter on the pipeline connecting the insulation coil and the nitrogen temporary storage tank is stable, it means that the insulation coil is full of nitrogen, and then close the first air inlet valve, the second air inlet valve, and the first air pump;
[0039] S64. During the reaction, according to the pH value of the reaction solution, the aluminum silicate solution is continuously added to the reaction solution to maintain the pH value of the normal reaction; specifically, the second feed valve, the pump body, and the first liquid outlet valve are opened in sequence, and the aluminum silicate solution in the aluminum silicate tank enters the insulation coil from the inlet of the insulation coil, and the nitrogen in the insulation coil is pushed into the reactor, and nitrogen is introduced into the reactor to prevent oxidation reaction from occurring during the reaction;
[0040] Meanwhile, in the process of gradually adding the aluminum silicate solution in the aluminum silicate tank to the reaction solution, when it is detected that the reaction solution reaches a suitable pH value, the second feed valve, the pump body, and the first liquid outlet valve are closed; and the pressure value in the reactor is observed. If the pressure value is too high, the exhaust valve on the top of the reactor can be opened for exhaust;
[0041] S65, after the pH value adjustment is completed, the first air inlet valve, the second air inlet valve and the first air pump are reopened, and the nitrogen in the nitrogen storage tank enters the insulation coil along the inlet of the insulation coil. When the gas flow rate detected by the gas flow meter on the pipeline connecting the insulation coil and the nitrogen temporary storage tank is stable, it means that the insulation coil is full of nitrogen, and then the first air inlet valve and the second air inlet valve are closed;
[0042] S66, after the reaction is completed, the second feed valve, the pump body, and the first liquid outlet valve are opened again, and the aluminum silicate solution in the aluminum silicate tank is continued to be added to the reaction solution to ensure that the aluminum silicate in the reaction solution is in an excessive state at the end of the reaction; at the same time, a viscosity reducer is added to the reaction solution from the liquid adding port on the top of the reactor;
[0043] S67, after the aluminum silicate in the reaction solution is in an excess state, the reaction solution is filtered, and the filter valve, the circulation pump body, and the liquid return valve are opened; the filtered aluminum silicate solution is recovered and transported to an aluminum silicate tank for storage; then the filter valve, the circulation pump body, and the liquid return valve are closed, and the feed valve is opened to recover the product magnesium silicate;
[0044] S68, open the air outlet valve and the second air pump to recover the nitrogen in the nitrogen temporary storage tank and store it in the nitrogen storage tank.
[0045] A low-alkali, low-viscosity magnesium silicate preparation process, a preparation device, and a working method of the device provided in an embodiment of the present invention have the following beneficial effects:
[0046] 1. The aluminum silicate solution is used as both a silicon source and a pH regulator, which does not require additional consumption of the pH regulator and also enables the preparation of low-alkalinity magnesium silicate, thereby reducing the cost of raw materials and simplifying the production process;
[0047] 2. The reaction raw materials in the present invention only need aluminum silicate solution, magnesium oxide solution and viscosity reducer, which reduces the types of raw materials and simplifies the supply chain management, thereby reducing the procurement cost and inventory management cost;
[0048] 3. The solution after the reaction is an excess aluminum silicate solution, which can be recovered and reused after filtration, which can save the consumption of raw materials and reduce the cost of raw materials;
[0049] 4. The product magnesium silicate will form suspended solid particles in the reaction solution. The magnesium silicate precipitate usually has a certain degree of adhesion and will adhere to the inner wall of the reactor. If the heating coil is set on the inner wall of the reactor, it will affect the cleaning of the inner wall of the reactor. To facilitate the cleaning of the inner wall of the reactor, the heating coil is set outside the reactor. When the stirrer is working, the scraper on the stirrer can be used to scrape and clean the inner wall of the reactor.
[0050] 5. The heating coil is set to a rectangular cross-section structure. When the heating coil is wrapped around the reactor, the rectangular cross-section heating coil increases the contact area between the heating coil and the reactor, thereby improving the heat exchange efficiency;
[0051] 6. An insulating coil is arranged around the outside of the heating coil. One of the functions of the insulating coil is to insulate and prevent the heating coil from directly contacting the outside air, causing heat spillover and waste. The insulating coil is filled with nitrogen. The nitrogen has a low convection movement inside, which can reduce the heat transfer rate and has good insulation performance. In addition, the reactor is provided with an insulating jacket on the outside of the insulating coil, and the insulating jacket is filled with insulation materials to further reduce heat spillover.
[0052] 7. In order to smoothly deliver the nitrogen in the nitrogen storage tank to the heating coil, a nitrogen temporary storage tank is added as a pressure balance tank. The nitrogen temporary storage tank is usually not filled with nitrogen or is in a negative pressure state. The nitrogen in the nitrogen storage tank can smoothly flow from the nitrogen storage tank to the nitrogen temporary storage tank with the help of the high pressure environment in the tank body and the first air pump;
[0053] 8. When adding aluminum silicate solution to the reaction solution to adjust the reaction pH range, the nitrogen in the insulation coil can be emptied, and the insulation coil is used as a conveying pipe and preheating pipe for the aluminum silicate solution. The aluminum silicate solution is preheated with the help of the heat in the insulation coil, which improves the thermal energy utilization rate and does not need to add preheating equipment to the aluminum silicate tank separately, thereby reducing the equipment cost; and the nitrogen emptied from the insulation coil is discharged into the reactor and can be used as a protective gas for the reaction;
[0054] 9. The cross section of the heat insulation coil is designed to be rectangular. In this way, when the heat insulation coil is used as a conveying pipe and preheating pipe for aluminum silicate solution, the heat insulation coil and the heating coil can have better surface contact, thereby improving the heat exchange efficiency. In addition, the walls of adjacent heat insulation coils are arranged close to the wall to form a nearly complete shielding surface, which can provide better heat insulation.
[0055] 10. After the reaction is completed, not only can the aluminum silicate solution be recovered, but the present invention also adds a nitrogen recovery system. The nitrogen in the nitrogen temporary storage tank is driven by the second air pump and returns to the nitrogen storage tank, thereby improving the utilization rate of nitrogen and reducing the reaction cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a structural schematic diagram of the low-alkali and low-viscosity magnesium silicate preparation device of the present invention;
[0057] Figure 2 This is a structural schematic diagram of the angle 1 at which the heating coil and the insulation coil are connected in the present invention;
[0058] Figure 3 It is a structural schematic diagram of the angle 2 of connecting the heating coil and the heat insulation coil in the present invention;
[0059] Figure 4 This is a structural schematic diagram of the stirrer at angle 1 in the present invention;
[0060] Figure 5 This is a schematic diagram of the structure of the agitator angle 2 in the present invention. DETAILED DESCRIPTION
[0061] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.
[0062] In view of the problems mentioned in the above background technology, the embodiment of the present invention provides a low-alkali and low-viscosity magnesium silicate preparation process, a preparation device and a working method of the device to solve the above technical problems. The technical solution is as follows:
[0063] Embodiment 1.
[0064] A low-alkali and low-viscosity magnesium silicate preparation process, comprising:
[0065] S1, respectively preparing aluminum silicate solution and magnesium oxide solution;
[0066] Among them, aluminum silicate solution is used as silicon source and pH regulator in the reaction, and magnesium oxide solution is used as magnesium source in the reaction;
[0067] S2, gradually adding the magnesium oxide solution to the aluminum silicate solution, so that the magnesium oxide solution reacts with the aluminum silicate solution to generate magnesium silicate;
[0068] S3. During the reaction, according to the pH value of the reaction solution, the aluminum silicate solution is gradually added to the reaction solution to maintain the reaction pH value range; the pH value range is controlled between 8.5-10;
[0069] S4. After the reaction is completed, continue to add aluminum silicate solution to the reaction solution to ensure that aluminum silicate is in excess in the reaction solution at the end of the reaction; at the same time, add a viscosity reducer to the reaction solution;
[0070] S5. After the aluminum silicate in the reaction solution is in an excess state, the reaction solution is filtered and the reaction filtrate is recovered; at the same time, the magnesium silicate removed from the reaction solution is recovered.
[0071] The low-alkali and low-viscosity magnesium silicate preparation process designed by the present invention has the following technical advantages:
[0072] 1. The aluminum silicate solution is used as both a silicon source and a pH regulator, which does not require additional consumption of the pH regulator and also enables the preparation of low-alkalinity magnesium silicate, thereby reducing the cost of raw materials and simplifying the production process;
[0073] 2. The reaction raw materials in the present invention only need aluminum silicate solution, magnesium oxide solution and viscosity reducer, which reduces the types of raw materials and simplifies the supply chain management, thereby reducing the procurement cost and inventory management cost;
[0074] 3. The solution after the reaction is excess aluminum silicate solution, which can be recovered and reused after filtration, which can save raw material consumption and reduce raw material costs.
[0075] Example 2, see Figure 1-Figure 5 .
[0076] A preparation device for low-alkali and low-viscosity magnesium silicate; comprising:
[0077] Reactor 1, aluminum silicate tank 2, nitrogen storage tank 3 and nitrogen temporary storage tank 4;
[0078] The first discharge port of the aluminum silicate tank 2 is connected to the aluminum silicate inlet of the reactor 1 through a pipeline; the first feed valve 7 is connected in series to the pipeline connecting the first discharge port of the aluminum silicate tank 2 and the aluminum silicate inlet of the reactor 1;
[0079] A heating coil 1-2 is arranged around the outer peripheral wall of the reactor 1, and the cross section of the heating coil 1-2 is rectangular; the hot water inlet of the heating coil 1-2 is located at one side of the bottom of the reactor 1, and the hot water outlet of the heating coil 1-2 is located at one side of the top of the reactor 1;
[0080] A hot water inlet valve 12 is provided at the hot water inlet of the heating coil 1-2, and a hot water outlet valve 16 is provided at the hot water outlet of the heating coil 1-2;
[0081] The outer side of the heating coil 1-2 is surrounded by a heat-insulating coil 1-3; the cross section of the heat-insulating coil 1-3 is rectangular, and the pipe walls of adjacent heat-insulating coils are arranged close to the wall;
[0082] The second discharge port of the aluminum silicate tank 2 and the first nitrogen outlet of the nitrogen storage tank 3 are respectively connected to the upper straight port and the lower straight port of the first three-way pipe 10, and the branch port of the first three-way pipe 10 is connected to the inlet of the insulation coil 1-3;
[0083] The second feed valve 8 and the pump body 9 are connected in series to the pipeline connecting the second discharge port of the aluminum silicate tank 2 and the upper straight port of the first three-way pipe 10; the first air inlet valve 11 is connected in series to the pipeline connecting the first nitrogen outlet of the nitrogen storage tank 3 and the lower straight port of the first three-way pipe 10;
[0084] The first nitrogen inlet of the nitrogen temporary storage tank 4 and the outlet of the heat insulation coil 1-3 are respectively connected to the upper straight port and the lower straight port of the second three-way pipe 26; the branch port of the second three-way pipe 26 is connected to the spray pipe 18 arranged in the reactor 1 through a pipeline;
[0085] The second air inlet valve 14, the first air pump 15, and the gas flow meter (not shown in the figure) are connected in series to the pipeline connecting the first nitrogen inlet port of the nitrogen temporary storage tank 4 and the upper straight port of the second three-way pipe 26; the first liquid outlet valve 17 is connected in series to the pipeline connecting the branch port of the second three-way pipe 26 and the spray pipe 18;
[0086] The second nitrogen outlet of the nitrogen temporary storage tank 4 is connected to the second nitrogen inlet of the nitrogen storage tank 3 through a pipeline, and the pipeline connecting the second nitrogen outlet of the nitrogen temporary storage tank 4 and the second nitrogen inlet of the nitrogen storage tank 3 is connected in series with the outlet valve 29 and the second air pump 19;
[0087] The discharge port at the bottom of the reactor 1 is connected to the upper straight port of the third three-way pipe 22, the lower straight port of the third three-way pipe 22 is connected to the discharge valve 20, and the branch port of the third three-way pipe 22 is connected to the liquid inlet of the aluminum silicate tank 2 through a pipeline; the pipeline connecting the branch port of the third three-way pipe 22 and the liquid inlet of the aluminum silicate tank 2 is connected in series with the filter valve 21, the circulation pump body 23, and the liquid return valve 25;
[0088] The top of the reactor 1 is provided with a liquid adding port 1a and an exhaust valve.
[0089] In this embodiment, a filter 27 is connected in series to the pipeline connecting the branch of the third three-way pipe 22 and the liquid inlet of the aluminum silicate tank 2; an agitator 5, a thermometer 6, and a pH sensor are provided inside the reactor 1; a sight glass 13 is connected in series to the pipeline connected in series to the first liquid outlet valve 17; the sight glass 13 can observe whether there is aluminum silicate solution entering the reactor 1.
[0090] In this embodiment, a heat insulating jacket 1 - 1 is provided on the outside of the heat insulating coil 1 - 3 on the reactor 1 , and the heat insulating jacket 1 - 1 is filled with heat insulating material.
[0091] The low-alkali and low-viscosity magnesium silicate preparation device designed by the present invention has the following technical advantages when preparing magnesium silicate:
[0092] 1. The product magnesium silicate will form suspended solid particles in the reaction solution. The magnesium silicate precipitate usually has a certain degree of adhesion and will adhere to the inner wall of the reactor 1. If the heating coil 1-2 is arranged on the inner wall of the reactor 1, it will affect the cleaning of the inner wall of the reactor 1. In order to facilitate the cleaning of the inner wall of the reactor 1, the heating coil 1-2 is arranged outside the reactor 1. When the stirrer 5 is working, the scraper 5-4 on the stirrer 5 can be used to conveniently scrape and clean the inner wall of the reactor 1;
[0093] 2. The heating coil 1-2 is set to a rectangular cross-section structure. When the heating coil 1-2 surrounds the reactor 1, the rectangular cross-section heating coil 1-2 increases the contact area between the heating coil 1-2 and the reactor 1, thereby improving the heat exchange efficiency;
[0094] 3. An insulating coil 1-3 is arranged around the outside of the heating coil 1-2. One of the functions of the insulating coil 1-3 is to provide insulation to prevent the heating coil 1-2 from directly contacting the outside air and causing heat spillover and waste; the insulating coil 1-3 is filled with nitrogen, and the nitrogen has a low convection movement inside, which can reduce the heat transfer rate and has good insulation performance; and the reactor 1 is provided with an insulating jacket 1-1 on the outside of the insulating coil 1-3, and the insulating jacket 1-1 is filled with insulation materials to further reduce heat spillover;
[0095] 4. In order to smoothly deliver the nitrogen in the nitrogen storage tank 3 to the heating coil 1-2, a nitrogen temporary storage tank 4 is added as a pressure balance tank. The nitrogen temporary storage tank 4 is usually not filled with nitrogen or is in a negative pressure state. The nitrogen in the nitrogen storage tank 3 can smoothly flow from the nitrogen storage tank 3 to the nitrogen temporary storage tank 4 with the help of the high-pressure environment in the tank body and the first air pump 15;
[0096] 5. When adding aluminum silicate solution to the reaction solution to adjust the reaction pH range, the nitrogen in the insulation coil 1-3 can be emptied, and the insulation coil 1-3 can be used as a conveying pipe and preheating pipe for the aluminum silicate solution. The aluminum silicate solution is preheated with the heat in the insulation coil 1-3, thereby improving the thermal energy utilization rate, and there is no need to add a separate preheating device to the aluminum silicate tank 2, thereby reducing the equipment cost; and the nitrogen emptied from the insulation coil 1-3 is discharged into the reactor 1 and can be used as a protective gas for the reaction;
[0097] It should be noted that if the aluminum silicate solution without preheating is directly added to the reactor 1, the overall temperature of the reaction liquid may be reduced, thereby affecting the reaction rate or causing the reaction to stagnate, and further affecting the yield and quality of the product; at the same time, if the temperature of the added aluminum silicate solution is low, it may cause local heat release in the reaction liquid, resulting in an increase in temperature or an increase in pressure in the reactor, thereby causing safety hazards;
[0098] 6. The cross section of the heat insulation coil 1-3 is designed to be rectangular. In this way, when the heat insulation coil 1-3 is used as a conveying pipe and a preheating pipe for the aluminum silicate solution, the heat insulation coil 1-3 and the heating coil 1-2 can have better surface contact, thereby improving the heat exchange efficiency; and the pipe walls of adjacent heat insulation coils are arranged close to the wall to form a nearly complete shielding surface, which can better insulate;
[0099] 7. After the reaction is completed, not only the aluminum silicate solution can be recovered, but the present invention also adds a nitrogen recovery system. The nitrogen in the nitrogen temporary storage tank 4 is driven by the second air pump 19 and returns to the nitrogen storage tank 3, thereby improving the utilization rate of nitrogen and reducing the reaction cost.
[0100] In this embodiment, the stirrer 5 includes a main stirring shaft 5-1, an upper stirring blade 5-2, a lower stirring blade 5-3, a scraper 5-4, a synchronous gear 5-5, a driving gear 5-6, an auxiliary stirring shaft 5-7, and a stirring blade 5-9;
[0101] The stirring shaft 5-1 is located in the reactor 1 and is vertically rotatably connected to the reactor 1;
[0102] The upper stirring blade 5-2 and the lower stirring blade 5-3 are arranged at intervals in the upper and lower parts, the upper stirring blade 5-2 is fixed to the upper half of the stirring shaft 5-1, and the lower stirring blade 5-3 is fixed to the lower half of the stirring shaft 5-1;
[0103] The scraper 5-4 includes two scrapers 5-4, which are respectively fixedly connected to the ends of the upper stirring blade 5-2 and the lower stirring blade 5-3 on the same side;
[0104] The synchronous gear 5-5 is fixed on the main stirring shaft 5-1, and the synchronous gear 5-5 is located above the upper stirring blade 5-2;
[0105] The auxiliary stirring shaft 5-7 includes two auxiliary stirring shafts 5-7, which are located on both sides of the stirring shaft 5-1. The upper and lower ends of the auxiliary stirring shaft 5-7 are rotatably connected to the upper stirring blade 5-2 and the lower stirring blade 5-3 respectively, and the upper end of the auxiliary stirring shaft 5-7 protrudes upward outside the upper stirring blade 5-2;
[0106] The driving gears 5-6 include two driving gears 5-6, which are respectively fixed at the upper ends of the auxiliary stirring shafts 5-7; the two driving gears 5-6 are respectively meshed with the synchronous gears 5-5 for transmission; and a plurality of groups of stirring blades 5-9 are arranged on each auxiliary stirring shaft 5-7.
[0107] When adding aluminum silicate solution to the reaction solution to adjust the reaction pH range, in order to ensure the normal reaction, the aluminum silicate solution needs to be quickly and evenly mixed in the reaction solution. The upper stirring blades 5-2 and lower stirring blades 5-3 arranged above and below can stir the upper and lower layers of the reaction solution; the scrapers 5-4 on both sides can not only stir the left and right sides of the reaction solution, but also clean and scrape off the magnesium silicate adhering to the inner wall of the reactor 1; the two auxiliary stirring shafts 5-7 and multiple groups of stirring blades 5-9 arranged in the middle increase the number of stirring blades and mixing strength in conventional agitators, which can improve the mixing ability of the reaction solution and mix the reaction materials in multiple directions.
[0108] Example 3, see Figure 1-Figure 5 .
[0109] A working method of a low-alkali and low-viscosity magnesium silicate preparation device comprises the following steps:
[0110] S61, respectively prepare an aluminum silicate solution and a magnesium oxide solution, the aluminum silicate solution is stored in the aluminum silicate tank 2; the magnesium oxide solution is stored in a temporary storage tank; open the first feed valve 7, and transport a certain amount of aluminum silicate solution from the aluminum silicate tank 2 to the reactor 1 as a silicon source and pH adjuster in the reaction; then close the first feed valve 7;
[0111] S62, adding the magnesium oxide solution in the temporary storage tank into the reactor 1 through the liquid adding port 1a on the reactor 1 to react; and introducing hot water from the hot water inlet of the heating coil 1-2 to heat the material in the reactor 1;
[0112] S63, during the reaction process, close the first liquid outlet valve 17; open the first air inlet valve 11, the second air inlet valve 14, and the first air pump 15 in sequence (the purpose of opening the first air inlet valve 11, the second air inlet valve 14, and the first air pump 15 is to form a passage between the nitrogen storage tank 3, the insulation coil 1-3, and the nitrogen temporary storage tank 4), and the nitrogen in the nitrogen storage tank 3 enters the insulation coil 1-3 along the inlet of the insulation coil 1-3. When the gas flow rate detected by the gas flow meter on the pipeline connecting the insulation coil 1-3 and the nitrogen temporary storage tank 4 is stable, it means that the insulation coil 1-3 is full of nitrogen, and then close the first air inlet valve 11, the second air inlet valve 14, and the first air pump 15;
[0113] S64. During the reaction, according to the pH value of the reaction solution, aluminum silicate solution is continuously added to the reaction solution to maintain the pH value of the normal reaction; specifically, the second feed valve 8, the pump body 9, and the first liquid outlet valve 17 are opened in sequence (the purpose of opening the second feed valve 8, the pump body 9, and the first liquid outlet valve 17 is to form a passage between the aluminum silicate tank 2, the insulation coil 1-3, and the spray pipe 18), and the aluminum silicate solution in the aluminum silicate tank 2 enters the insulation coil 1-3 from the inlet of the insulation coil 1-3, and the nitrogen in the insulation coil 1-3 is pushed into the reactor 1 through the spray pipe 18. The nitrogen introduced into the reactor 1 can prevent oxidation reaction from occurring during the reaction process;
[0114] Meanwhile, in the process of gradually adding the aluminum silicate solution in the aluminum silicate tank 2 to the reaction solution, when it is detected that the reaction solution reaches a suitable pH value, the second feed valve 8, the pump body 9, and the first liquid outlet valve 17 are closed; and the pressure value in the reactor 1 is observed. If the pressure value is too large, the exhaust valve at the top of the reactor can be opened to exhaust the gas;
[0115] S65, after the pH value adjustment is completed, the first air inlet valve 11, the second air inlet valve 14 and the first air pump 15 are reopened, and the nitrogen in the nitrogen storage tank 3 enters the insulation coil 1-3 along the inlet of the insulation coil 1-3. When the gas flow rate detected by the gas flow meter on the pipeline connecting the insulation coil 1-3 and the nitrogen temporary storage tank 4 is stable, it means that the insulation coil 1-3 is full of nitrogen, and then the first air inlet valve 11 and the second air inlet valve 14 are closed;
[0116] S66, after the reaction is completed, the second feed valve 8, the pump body 9, and the first liquid outlet valve 17 are opened again, and the aluminum silicate solution in the aluminum silicate tank 2 is continued to be added to the reaction solution to ensure that the aluminum silicate in the reaction solution is in an excessive state at the end of the reaction; at the same time, a viscosity reducer is added to the reaction solution from the liquid adding port 1a at the top of the reactor 1;
[0117] S67, after the aluminum silicate in the reaction solution is in an excessive state, the reaction solution is filtered, and the filter valve 21, the circulation pump body 23, and the liquid return valve 25 are opened (the purpose of opening the filter valve 21, the circulation pump body 23, and the liquid return valve 25 is to form a passage between the reactor 1 and the aluminum silicate tank 2); the filtered aluminum silicate solution is recovered and transported to the aluminum silicate tank 2 for storage; then the filter valve 21, the circulation pump body 23, and the liquid return valve 25 are closed, and the feed valve 20 is opened to recover the product magnesium silicate;
[0118] S68, opening the air outlet valve 29 and the second air pump 19, and recovering the nitrogen in the nitrogen temporary storage tank 4 to the nitrogen storage tank 3 for storage.
[0119] The device embodiments described above are merely illustrative, wherein the units described as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, and may be located in one place or distributed over multiple network units. Some or all of the modules may be selected according to actual needs to achieve the purpose of the solution of this embodiment.
[0120] In the present invention, unless otherwise clearly stipulated and limited, the terms such as "installation", "setting", "connection", "fixation" and "screw-on" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integrated connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of the components or the interaction relationship between the components. Unless otherwise clearly defined, for ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances.
[0121] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.
Claims
1. A process for preparing low-alkali and low-viscosity magnesium silicate, characterized in that: include: S1, respectively preparing aluminum silicate solution and magnesium oxide solution; Among them, aluminum silicate solution is used as silicon source and pH regulator in the reaction, and magnesium oxide solution is used as magnesium source in the reaction; S2, gradually adding the magnesium oxide solution to the aluminum silicate solution, so that the magnesium oxide solution reacts with the aluminum silicate solution to generate magnesium silicate; S3. During the reaction, according to the pH value of the reaction solution, the aluminum silicate solution is gradually added to the reaction solution to maintain the reaction pH value range; the pH value range is controlled between 8.5-10; S4. After the reaction is completed, continue to add aluminum silicate solution to the reaction solution to ensure that aluminum silicate is in excess in the reaction solution at the end of the reaction; at the same time, add a viscosity reducer to the reaction solution; S5. After the aluminum silicate in the reaction solution is in an excess state, the reaction solution is filtered and the reaction filtrate is recovered; at the same time, the magnesium silicate removed from the reaction solution is recovered.
2. A preparation device for low-alkali and low-viscosity magnesium silicate; characterized in that: include: Reactor, aluminum silicate tank, nitrogen storage tank and nitrogen temporary storage tank; The first discharge port of the aluminum silicate tank is connected to the aluminum silicate inlet of the reactor through a pipeline; the first feed valve is connected in series to the pipeline connecting the first discharge port of the aluminum silicate tank and the aluminum silicate inlet of the reactor; A heating coil is arranged around the outer wall of the reactor, and the cross section of the heating coil is rectangular; the hot water inlet of the heating coil is located at one side of the bottom of the reactor, and the hot water outlet of the heating coil is located at one side of the top of the reactor; An insulating coil is arranged around the outside of the heating coil; the cross section of the insulating coil is rectangular, and the pipe walls of adjacent insulating coils are arranged close to the wall; The second discharge port of the aluminum silicate tank and the first nitrogen outlet of the nitrogen storage tank are respectively connected to the upper straight port and the lower straight port of the first three-way pipe, and the branch port of the first three-way pipe is connected to the inlet of the insulation coil; A second feed valve and a pump body are connected in series to the pipeline connecting the second discharge port of the aluminum silicate tank and the upper straight port of the first three-way pipe; a first air inlet valve is connected in series to the pipeline connecting the first nitrogen outlet of the nitrogen storage tank and the lower straight port of the first three-way pipe; The first nitrogen inlet of the nitrogen temporary storage tank and the outlet of the heat-insulating coil are respectively connected to the upper straight port and the lower straight port of the second three-way pipe; the branch port of the second three-way pipe is connected to the spray pipe arranged in the reactor through a pipeline; The second air inlet valve, the first air pump, and the gas flow meter are connected in series to the pipeline connecting the first nitrogen inlet of the nitrogen temporary storage tank and the upper straight port of the second three-way pipe; the first liquid outlet valve is connected in series to the pipeline connecting the branch port of the second three-way pipe and the spray pipe; The second nitrogen outlet of the nitrogen temporary storage tank is connected to the second nitrogen inlet of the nitrogen storage tank through a pipeline, and the pipeline connecting the second nitrogen outlet of the nitrogen temporary storage tank and the second nitrogen inlet of the nitrogen storage tank is connected in series with an outlet valve and a second air pump; The discharge port at the bottom of the reactor is connected to the upper straight port of the third three-way pipe, the lower straight port of the third three-way pipe is connected to the discharge valve, and the branch port of the third three-way pipe is connected to the liquid inlet of the aluminum silicate tank through a pipeline; the pipeline connecting the branch port of the third three-way pipe and the liquid inlet of the aluminum silicate tank is connected in series with a filter valve, a circulation pump body, and a liquid return valve; Wherein, a liquid adding port and an exhaust valve are arranged on the top of the reactor.
3. The preparation device of low-alkali and low-viscosity magnesium silicate according to claim 2, characterized in that: A filter is connected in series to the pipeline connecting the branch of the third three-way pipe and the liquid inlet of the aluminum silicate tank; a stirrer, a thermometer and a pH sensor are arranged inside the reactor; and a sight glass is connected in series to the pipeline connected in series to the first liquid outlet valve.
4. The preparation device of low-alkali and low-viscosity magnesium silicate according to claim 2, characterized in that: A heat-insulating jacket is arranged on the outside of the heat-insulating coil on the reactor, and the heat-insulating jacket is filled with heat-insulating materials.
5. The preparation device of low-alkali and low-viscosity magnesium silicate according to claim 3, characterized in that: The agitator includes a main agitator shaft, an upper agitator blade, a lower agitator blade, a scraper, a synchronous gear, a driving gear, an auxiliary agitator shaft, and agitator blades; The stirring shaft is located in the reactor and is vertically rotatably connected to the reactor; The upper stirring blade and the lower stirring blade are arranged at intervals in the upper and lower parts, the upper stirring blade is fixed on the upper half of the stirring shaft, and the lower stirring blade is fixed on the lower half of the stirring shaft; The scrapers include two, and the two scrapers are respectively fixedly connected to the ends of the upper stirring blade and the lower stirring blade on the same side; The synchronous gear is fixed on the main stirring shaft, and the synchronous gear is located above the upper stirring blade; The auxiliary stirring shafts include two, which are located on both sides of the stirring shaft, and the upper and lower ends of the auxiliary stirring shafts are rotatably connected to the upper stirring blade and the lower stirring blade respectively, and the upper ends of the auxiliary stirring shafts protrude upward outside the upper stirring blade; The driving gears include two, and the two driving gears are respectively fixed on the upper ends of the auxiliary stirring shaft; The two driving gears are respectively meshed with the synchronous gears for transmission; and a plurality of stirring blades are arranged on each auxiliary stirring shaft.
6. A working method of the low-alkali and low-viscosity magnesium silicate preparation device according to any one of claims 2 to 5, characterized in that: The following steps are involved: S61, respectively preparing an aluminum silicate solution and a magnesium oxide solution, wherein the aluminum silicate solution is stored in an aluminum silicate tank; the magnesium oxide solution is stored in a temporary storage tank; opening a first feed valve, and conveying a certain amount of aluminum silicate solution from the aluminum silicate tank to the reactor as a silicon source and a pH adjuster in the reaction; and then closing the first feed valve; S62, adding the magnesium oxide solution in the temporary storage tank into the reactor through the liquid adding port on the reactor to react; and introducing hot water from the hot water inlet of the heating coil to heat the materials in the reactor; S63, during the reaction process, close the first liquid outlet valve; open the first air inlet valve, the second air inlet valve, and the first air pump in sequence, and the nitrogen in the nitrogen storage tank enters the insulation coil along the inlet of the insulation coil. When the gas flow rate detected by the gas flow meter on the pipeline connecting the insulation coil and the nitrogen temporary storage tank is stable, it means that the insulation coil is full of nitrogen, and then close the first air inlet valve, the second air inlet valve, and the first air pump; S64. During the reaction, according to the pH value of the reaction solution, the aluminum silicate solution is continuously added to the reaction solution to maintain the pH value of the normal reaction; specifically, the second feed valve, the pump body, and the first liquid outlet valve are opened in sequence, and the aluminum silicate solution in the aluminum silicate tank enters the insulation coil from the inlet of the insulation coil, and the nitrogen in the insulation coil is pushed into the reactor through the spray pipe, and the nitrogen is introduced into the reactor to prevent oxidation reaction during the reaction; Meanwhile, in the process of gradually adding the aluminum silicate solution in the aluminum silicate tank to the reaction solution, when it is detected that the reaction solution reaches a suitable pH value, the second feed valve, the pump body, and the first liquid outlet valve are closed; and the pressure value in the reactor is observed. If the pressure value is too high, the exhaust valve on the top of the reactor can be opened for exhaust; S65, after the pH value adjustment is completed, the first air inlet valve, the second air inlet valve and the first air pump are reopened, and the nitrogen in the nitrogen storage tank enters the insulation coil along the inlet of the insulation coil. When the gas flow rate detected by the gas flow meter on the pipeline connecting the insulation coil and the nitrogen temporary storage tank is stable, it means that the insulation coil is full of nitrogen, and then the first air inlet valve and the second air inlet valve are closed; S66, after the reaction is completed, the second feed valve, the pump body, and the first liquid outlet valve are opened again, and the aluminum silicate solution in the aluminum silicate tank is continued to be added to the reaction solution to ensure that the aluminum silicate in the reaction solution is in an excessive state at the end of the reaction; at the same time, a viscosity reducer is added to the reaction solution from the liquid adding port on the top of the reactor; S67, after the aluminum silicate in the reaction solution is in an excess state, the reaction solution is filtered, and the filter valve, the circulation pump body, and the liquid return valve are opened; the filtered aluminum silicate solution is recovered and transported to an aluminum silicate tank for storage; then the filter valve, the circulation pump body, and the liquid return valve are closed, and the feed valve is opened to recover the product magnesium silicate; S68, open the air outlet valve and the second air pump to recover the nitrogen in the nitrogen temporary storage tank and store it in the nitrogen storage tank.
Citation Information
Patent Citations
Hydroxyl magnesium silicate nanotube wear-resistant material and preparation method thereof
CN103880027A
No title available
GB1250905A
Improvements in magnesium aluminium silicates and in their preparation
GB873506A
Cited By
Anti-oxidation device suitable for molybdenum-based alloy reaction kettle
CN120094531A
An anti-oxidation device suitable for a molybdenum-based alloy reaction kettle
CN120094531B