Method for preparing deep hypothermia cold storage material gadolinium oxysulfide microspheres
After calcining and plasma sintering a mixture of Gd2O3, sublimated sulfur and sodium carbonate, high-quality sulfur oxide microspheres were prepared by plasma spheroidization technology, which solved the spherical and surface finish of sulfur gadolinium oxide microspheres in the prior art. The problem has improved its application performance under deep and low temperature conditions.
Patent Information
- Application Number
- CN202410866887.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-01
AI Technical Summary
The prior art is difficult to prepare sulfur gadolinium oxide microspheres with high spherical shape and smooth surface, and their application under deep and low temperature conditions is limited by the difficulty in processing and forming materials and poor plasticity.
Gd2O3, sublimated sulfur and sodium carbonate were mixed and stirred and calcined, followed by discharge plasma sintering and mechanical crushing under vacuum. Finally, sulfur gadolinium oxide microspheres with particle sizes of 100-500μm were prepared by plasma spheroidization technology.
Successfully obtained sulfur gadolinium oxide microspheres with high spherical shape and smooth surface, which are suitable for deep and low-temperature cooling materials, improving the low-temperature specific heat capacity and cooling efficiency.
Smart Images

Figure CN118955132A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of deep-low temperature cold storage materials, and in particular to a method for preparing gadolinium oxysulfide microspheres. Background Art
[0002] As a mature refrigeration equipment in the field of low-temperature applications, the Gifford-McMahon (GM) refrigerator has been widely used based on its working principle of gas compression and expansion process. During the working cycle of the GM refrigerator, the gas working medium exchanges heat with the cold storage material to achieve the purpose of refrigeration. Therefore, the cold storage material becomes the key material that determines the working efficiency of the refrigerator.
[0003] Gadolinium oxysulfide (Gd2O2S) has a high specific heat capacity under deep cryogenic conditions and can store more heat at low temperatures. It is an excellent deep cryogenic cold storage material. In order to obtain the highest refrigeration efficiency, the cold storage material is usually required to be spherical particles with a particle size of 100-500μm, which not only ensures that the cold storage material has a sufficiently large contact area with the gas working medium, but also reduces the flow resistance with the working medium in the cold storage device. However, since gadolinium oxysulfide is a ceramic rare earth cold storage material, it has poor plasticity, is brittle, and has a high melting point, making it difficult to process and form. At present, there are only some related studies on the preparation of gadolinium oxysulfide powder in China, such as CN2021115747544 discloses a method for preparing gadolinium oxysulfide powder, and the obtained powder has a small and uniform particle size; CN2016800521400 discloses a method for manufacturing rare earth sulfur oxides (including gadolinium oxysulfide), which can obtain high-purity fine sulfur oxides. However, there are few reports on how to prepare gadolinium oxysulfide microspheres (particle size greater than 150 μm). Therefore, how to prepare gadolinium oxysulfide microspheres with high sphericity and smooth surface is an important problem that needs to be solved urgently, which is of great significance to the development of domestic deep cryogenic refrigerators. Summary of the invention
[0004] Technical issues
[0005] In view of the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a method for preparing gadolinium oxysulfide microspheres as a deep-cryogenic cold storage material, which can obtain spherical gadolinium oxysulfide microspheres with high sphericity and smooth surface.
[0006] Technical Solution
[0007] According to a first aspect of the present invention, there is provided a method for preparing gadolinium oxysulfide microspheres, comprising the following steps:
[0008] (S1) Gd2O3, sublimed sulfur and sodium carbonate are mixed and stirred to obtain a mixed powder, which is then calcined under a protective atmosphere, and then washed with dilute hydrochloric acid, alcohol and deionized water to obtain pure gadolinium oxysulfide powder;
[0009] (S2) pre-pressing the gadolinium oxysulfide powder obtained in step (S1) to obtain a green body, sintering the green body in a spark plasma sintering furnace under vacuum conditions to obtain a gadolinium oxysulfide block, and mechanically crushing and screening to obtain particles with a particle size of 100 to 500 μm;
[0010] (S3) Processing the gadolinium oxysulfide particles obtained in step (S2) into gadolinium oxysulfide microspheres using plasma spheroidization technology.
[0011] Preferably, the cleaning dilute hydrochloric acid is a 0.05-0.3 mol / L solution.
[0012] Preferably, the mass ratio of Gd2O3, S and sodium carbonate is 5:1.1-1.9:0.7-2.1, and more preferably, the mass ratio of Gd2O3, S and sodium carbonate is 5:1.5:1.4.
[0013] Preferably, the purity of Gd2O3 is above 99.9%.
[0014] Preferably, in step (S1), the protective atmosphere is argon or vacuum atmosphere.
[0015] Preferably, in step (S1), the calcination temperature is 1100°C to 1200°C, and the calcination time is 2 to 8 hours.
[0016] Preferably, the pre-pressing pressure is 10-15 MPa.
[0017] Preferably, in step (S2), spark plasma sintering is performed under the following conditions:
[0018] The pressure is 30-50 MPa;
[0019] The heating rate is 40-60℃ / min;
[0020] The highest temperature is 1200-1300℃;
[0021] The holding time at the highest temperature is at least 10 minutes.
[0022] Preferably, the powder particle size after crushing is between 100 and 500 μm; more preferably, gadolinium oxysulfide powder of about 250 μm is used.
[0023] Preferably, the power of the plasma spheroidization in step (S3) is 30 kW to 40 kW.
[0024] Preferably, the powder feeding rate during spheroidization in step (S3) is 3 g / min to 10 g / min, preferably 3 g / min to 6 g / min.
[0025] Preferably, the carrier gas flow rate during spheroidization in step (S3) is controlled at 1 to 3 slpm.
[0026] Preferably, the particle size of the obtained gadolinium oxysulfide microspheres is 100 to 300 μm.
[0027] According to a second aspect of the present invention, there is provided a gadolinium oxysulfide microsphere, which is obtained by the method for preparing gadolinium oxysulfide microsphere according to the present invention.
[0028] Preferably, the particle size of the gadolinium oxysulfide microspheres is 100 to 300 μm.
[0029] In view of the defects of the existing preparation technology, the present invention provides a method for preparing gadolinium oxysulfide microspheres. The gadolinium oxysulfide microspheres prepared by the method have high sphericity, smooth surface and large low-temperature specific heat. The microspheres are filled into a cold storage machine and can be used as a deep-low temperature cold storage material. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The X-ray diffraction pattern of gadolinium oxysulfide microspheres prepared according to Example 1 of the present invention is shown;
[0031] Figure 2 The scanning electron microscope image of gadolinium oxysulfide microspheres prepared according to Example 2 of the present invention is shown;
[0032] Figure 3 a and Figure 3 b are optical microscope photographs and SEM photographs showing the gadolinium oxysulfide microspheres prepared in Comparative Example 2, respectively.
[0033] Figure 3 c and Figure 3 d are optical microscope photographs and SEM photographs of the gadolinium oxysulfide microspheres prepared in Comparative Example 1, respectively.
[0034] Figure 3 e and Figure 3 f are an optical microscope photograph and a SEM photograph respectively showing the gadolinium oxysulfide microspheres prepared according to Example 4 of the present invention.
[0035] Figure 3 g and Figure 3 h are optical microscope photographs and SEM photographs respectively showing gadolinium oxysulfide microspheres prepared according to Example 3 of the present invention. DETAILED DESCRIPTION
[0036] The following is an explanation of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0037] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are intended to describe specific embodiments, rather than to limit the scope of protection of the present invention. The test methods in the following examples without specifying specific conditions are generally carried out under conventional conditions or under conditions recommended by the manufacturers.
[0038] When the embodiments give numerical ranges, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the grasp of the prior art by those skilled in the art and the record of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.
[0039] raw material
[0040] Gd2O3: Gadolinium oxide (Gd2O3) powder provided by Jiangxi Ganzhou Yttrium Energy New Materials Co., Ltd. has an average particle size of about 10 μm (purity of 99.9%);
[0041] equipment
[0042] Plasma spheroidization system, RF plasma powder making system from Canada TEKNA, model TekSphero-40kW Plasma System;
[0043] Plasma sintering furnace: LABOX-350 SPS spark plasma sintering device produced by SINTER LAND INC.;
[0044] Example 1
[0045] The deep-cryogenic cold storage material gadolinium oxysulfide microspheres are prepared according to the following steps:
[0046] (1) Take 20g of high-purity gadolinium oxide, 6g of sublimed sulfur powder, and 5.6g of anhydrous sodium sulfate, put them into a sealed quartz tube, mix them evenly, fill them with argon gas to protect the seal, and calcine them at 1100°C for 4h in an argon atmosphere in a muffle furnace. Subsequently, the calcined product is washed with 0.1mol / L dilute hydrochloric acid, anhydrous ethanol, and deionized water in sequence, and then vacuum-heated to 70°C in a drying oven and dried for 6h.
[0047] (2) The gadolinium oxysulfide powder prepared in step (1) is pre-pressed into a green body at a pressure of 10 MPa, and then the green body is placed in a vacuum plasma sintering furnace for sintering, the pressure is maintained at 40 MPa, the temperature is raised to 1200° C. at a heating rate of 50° C. / min, and then kept warm. After reaching the target temperature, the temperature is kept warm for 10 minutes to obtain a gadolinium oxysulfide block. Subsequently, the gadolinium oxysulfide block is crushed into irregular particles using a crusher, and the irregular particles with a particle size of 100 to 150 μm are sieved.
[0048] (3) The irregular particles obtained in step (2) were spheroidized by a plasma spheroidization system, with the spheroidization power set to 35 kW, the powder feeding rate set to 6 g / min, and the carrier gas flow rate set to 3 pslm, to obtain spherical gadolinium oxysulfide microspheres. The obtained gadolinium oxysulfide microspheres were single-phase.
[0049] like Figure 1 As shown, the XRD test results show that compared with the standard peaks of gadolinium oxysulfide, the product has all the standard peaks of gadolinium oxysulfide and no impurity peaks are generated.
[0050] The particle size is about 100μm, with high sphericity and smooth surface.
[0051] Example 2
[0052] The deep-cryogenic cold storage material gadolinium oxysulfide microspheres are prepared according to the following steps:
[0053] (1) Take 20g of high-purity gadolinium oxide, 6g of sublimed sulfur powder, and 5.6g of anhydrous sodium sulfate, put them into a sealed quartz tube, mix them evenly, fill them with argon gas to protect the seal, and calcine them at 1100°C for 4h in an argon atmosphere in a muffle furnace. Subsequently, the calcined product is washed with 0.1mol / L dilute hydrochloric acid, anhydrous ethanol, and deionized water in sequence, and then vacuum-heated to 70°C in a drying oven and dried for 6h.
[0054] (2) The gadolinium oxysulfide powder prepared in step (1) is pressed into a green body at a pressure of 15 MPa, and then the green body is placed in a vacuum plasma sintering furnace for sintering, the pressure is maintained at 40 MPa, the temperature is raised to 1200° C. at a heating rate of 50° C. / min, and then kept warm. After reaching the target temperature, the temperature is kept warm for 20 minutes to obtain a gadolinium oxysulfide block. Subsequently, the gadolinium oxysulfide block is crushed into irregular particles using a crusher, and the irregular particles with a particle size of 150 to 200 μm are sieved.
[0055] (3) The irregular particles obtained in step (2) were spheroidized by a plasma spheroidization system, the spheroidization power was set to 38KW, the powder feeding rate was set to 3 / min, and the carrier gas flow rate was set to 1plsm to obtain gadolinium oxysulfide microspheres. The obtained gadolinium oxysulfide microspheres were single-phase.
[0056] Figure 2The scanning electron microscope image of gadolinium oxysulfide microspheres prepared according to Example 2 of the present invention is shown as follows: Figure 2 As shown, the particle size is about 150 μm, with high sphericity and smooth surface.
[0057] Example 3
[0058] The deep-cryogenic cold storage material gadolinium oxysulfide microspheres are prepared according to the following steps:
[0059] (1) Take 20g of high-purity gadolinium oxide, 6g of sublimed sulfur powder, and 5.6g of anhydrous sodium sulfate, put them into a sealed quartz tube, mix them evenly, fill them with argon gas to protect the seal, and calcine them at 1100°C for 4h in an argon atmosphere in a muffle furnace. Subsequently, the calcined product is washed with 0.1mol / L dilute hydrochloric acid, anhydrous ethanol, and deionized water in sequence, and then vacuum-heated to 70°C in a drying oven and dried for 6h.
[0060] (2) The gadolinium oxysulfide powder prepared in step (1) is pressed into a green body at a pressure of 10 MPa, and then the green body is placed in a vacuum plasma sintering furnace for sintering, the pressure is maintained at 40 MPa, the temperature is increased to 1200° C. at a heating rate of 50° C. / min, and then kept warm. After reaching the target temperature, the temperature is kept warm for 10 minutes to obtain a gadolinium oxysulfide block. Subsequently, the gadolinium oxysulfide block is crushed into irregular particles using a crusher, and the irregular particles with a particle size of 100 to 300 μm are sieved.
[0061] (3) The irregular particles obtained in step (2) were spheroidized by a plasma spheroidization system, with the spheroidization power set to 40 kW, the powder feeding rate set to 3 g / min, and the carrier gas flow rate set to 1 pslm, to obtain spherical gadolinium oxysulfide microspheres. The obtained gadolinium oxysulfide microspheres were single-phase.
[0062] The optical microscope and SEM images of the prepared gadolinium oxysulfide microspheres can be found in Figure 3 g and Figure 3 h.
[0063] Example 4
[0064] The deep-cryogenic cold storage material gadolinium oxysulfide microspheres are prepared according to the following steps:
[0065] (1) Take 20g of high-purity gadolinium oxide, 6g of sublimed sulfur powder, and 5.6g of anhydrous sodium sulfate, put them into a sealed quartz tube, mix them evenly, fill them with argon gas to protect the seal, and calcine them at 1100°C for 4h in an argon atmosphere in a muffle furnace. Subsequently, the calcined product is washed with 0.1mol / L dilute hydrochloric acid, anhydrous ethanol, and deionized water in sequence, and then vacuum-heated to 70°C in a drying oven and dried for 6h.
[0066] (2) The gadolinium oxysulfide powder prepared in step (1) is pressed into a green body at a pressure of 10 MPa, and then the green body is placed in a vacuum plasma sintering furnace for sintering, the pressure is maintained at 40 MPa, the temperature is increased to 1200° C. at a heating rate of 50° C. / min, and then kept warm. After reaching the target temperature, the temperature is kept warm for 10 minutes to obtain a gadolinium oxysulfide block. Subsequently, the gadolinium oxysulfide block is crushed into irregular particles using a crusher, and the irregular particles with a particle size of 100 to 300 μm are sieved.
[0067] (3) The irregular particles obtained in step (2) were spheroidized by a plasma spheroidization system, with the spheroidization power set to 35 kW, the powder feeding rate set to 9 g / min, and the carrier gas flow rate set to 3 pslm, to obtain spherical gadolinium oxysulfide microspheres. The obtained gadolinium oxysulfide microspheres were single-phase.
[0068] The optical microscope and SEM images of the prepared gadolinium oxysulfide microspheres can be found in Figure 3 e and Figure 3 f.
[0069] Comparative Example 1
[0070] The deep-cryogenic cold storage material gadolinium oxysulfide microspheres are prepared according to the following steps:
[0071] (1) Take 20g of high-purity gadolinium oxide, 6g of sublimed sulfur powder, and 5.6g of anhydrous sodium sulfate, put them into a sealed quartz tube, mix them evenly, fill them with argon gas to protect the seal, and calcine them at 1100°C for 4h in an argon atmosphere in a muffle furnace. Subsequently, the calcined product is washed with 0.1mol / L dilute hydrochloric acid, anhydrous ethanol, and deionized water in sequence, and then vacuum-heated to 70°C in a drying oven and dried for 6h.
[0072] (2) The gadolinium oxysulfide powder prepared in step (1) is pressed into a green body at a pressure of 10 MPa, and then the green body is placed in a vacuum plasma sintering furnace for sintering, the pressure is maintained at 40 MPa, the temperature is increased to 1200° C. at a heating rate of 50° C. / min, and then kept warm. After reaching the target temperature, the temperature is kept warm for 10 minutes to obtain a gadolinium oxysulfide block. Subsequently, the gadolinium oxysulfide block is crushed into irregular particles using a crusher, and the irregular particles with a particle size of 100 to 300 μm are sieved.
[0073] (3) The irregular particles obtained in step (2) were spheroidized by a plasma spheroidization system, with the spheroidization power set to 40 kW, the powder feeding rate set to 16 g / min, and the carrier gas flow rate set to 1 pslm, to obtain spherical gadolinium oxysulfide microspheres. The obtained gadolinium oxysulfide microspheres were single-phase.
[0074] The optical microscope and SEM images of the prepared gadolinium oxysulfide microspheres can be found in Figure 3 c and Figure 3 d.
[0075] Comparative Example 2
[0076] The deep-cryogenic cold storage material gadolinium oxysulfide microspheres are prepared according to the following steps:
[0077] (1) Take 20g of high-purity gadolinium oxide, 6g of sublimed sulfur powder, and 5.6g of anhydrous sodium sulfate, put them into a sealed quartz tube, mix them evenly, fill them with argon gas to protect the seal, and calcine them at 1100°C for 4h in an argon atmosphere in a muffle furnace. Subsequently, the calcined product is washed with 0.1mol / L dilute hydrochloric acid, anhydrous ethanol, and deionized water in sequence, and then vacuum-heated to 70°C in a drying oven and dried for 6h.
[0078] (2) The gadolinium oxysulfide powder prepared in step (1) is pressed into a green body at a pressure of 10 MPa, and then the green body is placed in a vacuum plasma sintering furnace for sintering, the pressure is maintained at 40 MPa, the temperature is increased to 1200° C. at a heating rate of 50° C. / min, and then kept warm. After reaching the target temperature, the temperature is kept warm for 10 minutes to obtain a gadolinium oxysulfide block. Subsequently, the gadolinium oxysulfide block is crushed into irregular particles using a crusher, and the irregular particles with a particle size of 100 to 300 μm are sieved.
[0079] (3) The irregular particles obtained in step (2) were spheroidized by a plasma spheroidization system, with the spheroidization power set to 40 kW, the powder feeding rate set to 33 g / min, and the carrier gas flow rate set to 1 pslm, to obtain spherical gadolinium oxysulfide microspheres. The obtained gadolinium oxysulfide microspheres were single-phase.
[0080] The optical microscope and SEM images of the prepared gadolinium oxysulfide microspheres can be found in Figure 3 a and Figure 3 b.
[0081] from Figure 3 It can be seen that when the powder feeding rate is 33g / min ( Figure 3 a and Figure 3 b), only a small amount of Gd2S particles become spherical Gd2S particles after plasma spheroidization, and most of the Gd2S particles are still irregular; when the powder feeding rate is reduced to 16 g / min, the spheroidization effect of Gd2S powder is slightly improved, but the spheroidization rate is still very low ( Figure 3 c and Figure 3 d); Continue to reduce the powder feeding rate to 9g / min, the number of spherical particles after plasma spheroidization increases ( Figure 3 e and Figure 3 f); Similarly, the unspheroidized particles are still in agglomerated state. Further reducing the powder feeding rate to 3g / min ( Figure 3 g and Figure 3h), the agglomeration of particles disappears, almost all of the gadolinium oxysulfide particles are spheroidized, and the spheroidization rate is as high as 95.18%, and the surface of the spherical gadolinium oxysulfide particles is smooth and well dispersed. Therefore, the spheroidization rate of the particles increases with the decrease of the powder feeding rate, and the spheroidization rate reaches the maximum when the powder feeding rate is 3g / min. Gadolinium oxysulfide, as a ceramic material, has a very high melting point, and it takes a lot of energy to completely melt the powder particles. As the powder feeding rate decreases, the number of particles passing through the torch per unit time decreases, and more energy is obtained during the spheroidization of the particles, which enables the irregular particles of gadolinium oxysulfide to obtain enough energy to be completely spheroidized.
Claims
1. A method for preparing gadolinium oxysulfide microspheres, comprising the following steps: (S1) Gd2O3, sublimed sulfur and sodium carbonate are mixed and stirred to obtain a mixed powder, which is then calcined under a protective atmosphere, and then washed with dilute hydrochloric acid, alcohol and deionized water to obtain pure gadolinium oxysulfide powder; (S2) pre-pressing the gadolinium oxysulfide powder obtained in step (S1) to obtain a green body, sintering the green body in a spark plasma sintering furnace under vacuum conditions to obtain a gadolinium oxysulfide block, and mechanically crushing and screening to obtain particles with a particle size of 100 to 500 μm; (S3) Processing the gadolinium oxysulfide particles obtained in step (S2) into gadolinium oxysulfide microspheres using plasma spheroidization technology.
2. The method for preparing gadolinium oxysulfide microspheres according to claim 1, wherein: The dilute hydrochloric acid for cleaning is a 0.05-0.3 mol / L solution.
3. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: The mass ratio of Gd2O3, S and sodium carbonate is 5:1.1-1.9:0.7-2.1, Preferably, the mass ratio of Gd2O3, S and sodium carbonate is 5:1.5:1.
4.
4. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: The purity of Gd2O3 is above 99.9%; and / or In step (S1), the protective atmosphere refers to an argon gas or vacuum atmosphere.
5. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: In step (S1), the calcination temperature is 1100°C to 1200°C, and the calcination time is 2 to 8 hours.
6. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: In step (S2), The pre-pressing pressure is 10-15 MPa; and / or Spark plasma sintering is carried out under the following conditions: The pressure is 30-50 MPa; The heating rate is 40-60℃ / min; The highest temperature is 1200-1300℃; The holding time at the highest temperature is at least 10 minutes.
7. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: Use gadolinium oxysulfide powder with a crushed powder particle size between 100 and 500 μm; preferably, use gadolinium oxysulfide powder with a particle size of about 250 μm.
8. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: The power of the plasma spheroidization in step (S3) is 30 kW to 40 kW; and / or The powder feeding rate during spheroidization in step (S3) is 3 g / min to 10 g / min.
9. The method for preparing gadolinium oxysulfide microspheres according to claim 1 or 2, wherein: The carrier gas flow rate during spheroidization in step (S3) is controlled to be 1 to 3 slpm.
10. Gadolinium oxysulfide microspheres obtained by the method for preparing gadolinium oxysulfide microspheres according to any one of claims 1 to 9, preferably, the gadolinium oxysulfide microspheres have a particle size of 100 to 300 μm.
Citation Information
Patent Citations
Method for producing rare earth oxysulfide, rare earth oxysulfide, and regenerator material
CN108025924A
Preparation method of gadolinium oxysulfide powder
CN114162847A
Indirect sulfur source preparation method of gadolinium oxysulfide scintillation ceramic powder
CN105800662A
Rare-earth cold storage material particles, refrigerator using same, superconducting magnet, inspection device, and cryopump
CN106715637A
Preparation method and application of nano gadolinium zirconate powder for plasma spraying
CN111777413A
Cited By
Gadolinium oxysulfide cold storage ceramic microspheres as well as preparation method and application thereof
CN120817804A
Gadolinium oxysulfide regenerative ceramic microspheres, and preparation method and application thereof
CN120817804B
Continuous preparation method of rare earth oxide / oxysulfide nano material with uniform particles
CN121735294A
Deep hypothermia cold storage material ErNi spherical particles and preparation method and application thereof
CN122605993A
Cold storage material, and preparation method therefor and use thereof
WO2026108235A1