Preparation method of semiconductor silicon carbide ceramic material

By using a mixed preparation method of high-purity carbon source and silicon particles in a vacuum environment, the melting and evaporation reaction of silicon carbide in a high-temperature induction furnace is solved, and the problems of low purity of silicon carbide and environmental pollution in the prior art are realized. The preparation of high-purity silicon carbide meets the needs of semiconductor ceramic materials.

CN118955144APending Publication Date: 2024-11-15SHANDONG SHENGNUO IND CO LTD

Patent Information

Application Number
CN202411011737.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing silicon carbide preparation methods have low purity due to the simple use of equipment, which causes environmental pollution and does not meet environmental protection requirements, and cannot meet the needs of high-purity silicon carbide in semiconductor ceramic boat manufacturing.

Method used

Under the protection of vacuum ambient gas, high-purity carbon source and high-purity silicon particles are used to prepare the reaction precursor, and melt and evaporate reactions are carried out in a high-temperature induction furnace to generate high-purity silicon carbide to avoid contamination of metal impurities.

Benefits of technology

The high-purity preparation of silicon carbide (purity can reach 99.995%) is achieved, which reduces environmental pollution and meets the needs of high-purity silicon carbide in semiconductor ceramic materials.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of silicon carbide, and discloses a preparation method of a semiconductor silicon carbide ceramic material, which comprises the following steps: S1, in a furnace body under the protection of gas in a vacuum environment; s2, sufficiently mixing the particles of the high-purity carbon source with the particles of the high-purity silicon to prepare a reaction precursor in a certain proportion; s3, melting and evaporating the silicon raw material in the reaction precursor in a high-temperature environment according to the step S2; s4, according to the step S3, the molten and evaporated silicon melt reacts with a high-purity carbon raw material to generate silicon carbide, a high-purity carbon source free of metal impurities is adopted to replace a petroleum coke carbon raw material in an existing preparation method, and due to the fact that the purity can reach 99.995% or above, and the impurity content of the silicon raw material is smaller than 100 ppm, the purity of the silicon raw material can reach 99.995% or above; according to the present invention, the silicon raw material is in the melting or evaporation gasification state during the carbonization reaction, the purity of the prepared silicon carbide is high and can achieve 99.995%, and the preparation method does not produce the metal ash content, avoids the environmental pollution, and has the large market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicon carbide preparation, in particular to a method for preparing semiconductor silicon carbide ceramic materials. Background Art

[0002] The existing method for preparing silicon carbide is to mix quartz sand raw material and petroleum coke raw material in proportion and prepare it by heating in an Acheson resistance furnace; these quartz sand and petroleum coke contain a large amount of metal impurity ash, and these impurities also undergo chemical reactions under high-temperature heating conditions, which also have a great impact on the purity of the silicon carbide itself, making the purity of the silicon carbide low and unable to meet the market demand for high-purity silicon carbide, resulting in it being unable to be used as a raw material in the manufacture of semiconductor ceramic wafer boats. The existing preparation method has many problems that need to be solved urgently.

[0003] At present, the existing silicon carbide is produced by simple equipment. This simple open-air equipment mass-produces silicon carbide with low purity, which will cause great pollution to the environment. It is low-priced and does not meet environmental protection requirements. Therefore, it does not meet the existing needs. In this regard, we have proposed a method for preparing semiconductor silicon carbide ceramic materials. Summary of the invention

[0004] The utility model provides a method for preparing semiconductor silicon carbide ceramic material, which has beneficial effects and solves the problem mentioned in the above background technology that the existing silicon carbide is produced by simple equipment, and such simple open-air equipment mass-produces silicon carbide with low purity, which will cause great pollution to the environment, is low in price, and does not meet environmental protection requirements.

[0005] The present invention provides the following technical solution: a method for preparing semiconductor silicon carbide ceramic material, comprising the following steps:

[0006] S1. Use the furnace body under the protection of hydrogen gas in a vacuum environment;

[0007] S2. Use high-purity carbon source particles and high-purity silicon particles to fully mix to prepare a reaction precursor in a certain ratio.

[0008] S3. According to S2, the silicon raw material in the reaction precursor is melted and evaporated in a high temperature environment;

[0009] S4. According to S3, the melted and evaporated silicon melt reacts with the high-purity carbon raw material to form silicon carbide.

[0010] As an optional scheme for the preparation method of semiconductor silicon carbide ceramic material described in the present invention, the particles of the high-purity carbon source and the particles of the high-purity silicon source are fully mixed to prepare a reaction precursor in a certain proportion, the carbon raw material content in the reaction precursor is 2-5, and the silicon raw material content in the reaction precursor is 7-10.

[0011] As an optional scheme for the method for preparing semiconductor silicon carbide ceramic material described in the present invention, the carbon-containing raw materials in the reaction precursor are high-purity carbon powder and graphite.

[0012] As an optional scheme for the method for preparing semiconductor silicon carbide ceramic material described in the present invention, the particle size of the mixed particles of high-purity carbon powder and graphite is 40-100 mesh.

[0013] As an optional solution for the method for preparing the semiconductor silicon carbide ceramic material described in the present invention, the purity of the high-purity carbon powder and graphite mixed particles is higher than 99.995%.

[0014] As an optional scheme for the method for preparing semiconductor silicon carbide ceramic material described in the present invention, the high-purity silicon source is set to high-purity quartz sand and high-purity silicon powder, and the impurity content of the high-purity quartz sand and the high-purity silicon powder is less than 100 ppm.

[0015] As an optional scheme for the method for preparing the semiconductor silicon carbide ceramic material described in the present invention, the particle size of the mixture of the high-purity silicon powder and the high-purity quartz sand is 100-150 meshes.

[0016] As an optional scheme for the preparation method of semiconductor silicon carbide ceramic material described in the present invention, the reaction position where the reaction precursor generates silicon carbide is in a crucible inside a high-temperature induction furnace, the crucible is a high-purity graphite crucible with boron carbide sprayed on the surface, the induction furnace is induction heated, and the maximum temperature in the induction furnace is set to 2500°C.

[0017] As an optional scheme for the preparation method of semiconductor silicon carbide ceramic material described in the present invention, the silicon raw material in the reaction precursor melts and evaporates in a high-temperature environment, the melted and evaporated silicon melt and gas react with the high-purity carbon raw material to generate silicon carbide, and the induction furnace is in a vacuum hydrogen protection state.

[0018] As an optional solution to the method for preparing semiconductor silicon carbide ceramic material described in the present invention, the heat source generator for the high-temperature environment of the melting and evaporation of the silicon raw material is induction coil heating.

[0019] This utility model has the following beneficial effects:

[0020] 1. The semiconductor ceramic crystal boat adopts a synthesis method of high-purity silicon carbide, and adopts a high-purity carbon source without metal impurities to replace the petroleum coke carbon raw material in the existing preparation method. Since the purity can reach more than 99.995%, the impurity content of the silicon raw material is less than 100ppm, and the silicon raw material is in a molten or evaporated gas state during the carburization reaction, the prepared silicon carbide has a high purity of 99.995%. This preparation method does not produce metal ash, avoids pollution to the environment, and has a large market prospect.

[0021] 2. The synthesis method of high-purity silicon carbide for the semiconductor ceramic wafer boat is as follows: the silicon raw material in the reaction precursor is melted and evaporated in a high-temperature environment, and the melted and evaporated silicon melt and gas react with the high-purity carbon raw material to generate silicon carbide. The induction furnace is in a vacuum hydrogen protection state, and the heat source generator of the high-temperature environment of the melted and evaporated silicon raw material is heated by an induction coil. At the same time, the preparation method of silicon carbide is realized by an electric induction furnace preparation device. In the furnace body protected by inert gas argon, the silicon raw material for producing silicon carbide is melted or evaporated in a high-temperature environment exceeding 2000°C, and the melted or evaporated silicon raw material reacts with the carbon raw material to generate silicon carbide. The silicon raw material in the high-temperature environment melts or evaporates, and reacts with the carbon raw material to generate silicon carbide. This method can efficiently prepare high-purity silicon carbide. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Embodiment 1: This embodiment is intended to promote the solution of the problem that the existing silicon carbide is produced by simple equipment. Such simple open-air equipment produces a large amount of silicon carbide with low purity, which will cause great pollution to the environment, is low in price, and does not meet environmental protection requirements. The preparation method of semiconductor silicon carbide ceramic material,

[0024] S1. Use the furnace body under the protection of hydrogen gas in a vacuum environment;

[0025] S2. Use high-purity carbon source particles and high-purity silicon particles to fully mix to prepare a reaction precursor in a certain ratio.

[0026] S3. According to S2, the silicon raw material in the reaction precursor is melted and evaporated in a high temperature environment;

[0027] S4. According to S3, the melted and evaporated silicon melt reacts with the high-purity carbon raw material to form silicon carbide.

[0028] The particles of high-purity carbon source and high-purity silicon source are fully mixed to prepare a reaction precursor of a certain ratio, wherein the carbon raw material in the reaction precursor is 2-5, and the silicon raw material in the reaction precursor is 7-10.

[0029] The carbon-containing raw materials in the reaction precursor are high-purity carbon powder and graphite. The particle size of the mixed particles of high-purity carbon powder and graphite is 40-100 meshes. The purity of the mixed particles of high-purity carbon powder and graphite is higher than 99.995%. The high-purity silicon source is set to high-purity quartz sand and high-purity silicon powder. The impurity content of the high-purity quartz sand and high-purity silicon powder is less than 100ppm. The particle size of the mixture particles of high-purity silicon powder and high-purity quartz sand is 100-150 meshes.

[0030] In this embodiment: in a furnace body protected by hydrogen gas in a vacuum environment, a high-purity silicon raw material for producing silicon carbide is melted or evaporated in a high-temperature environment exceeding 2000°C, and the melted or evaporated silicon raw material reacts with a high-purity carbon source to generate silicon carbide. Since the carbon source and the silicon source have very high purity and do not contain metal impurities, high-purity silicon carbide can be obtained, and the absence of metal impurities will not cause air pollution of metal ash.

[0031] Embodiment 2: This embodiment aims to promote the solution of the problem of using an electric induction furnace preparation device to melt or evaporate the silicon raw material for producing silicon carbide in a high temperature environment exceeding 2000°C in a furnace body protected by an inert gas argon. This embodiment is an improvement made on the basis of Embodiment 1. Specifically, the reaction position of the reaction precursor to generate silicon carbide is in a crucible in the high-temperature induction furnace body. The crucible is a high-purity graphite crucible with boron carbide sprayed on the surface. The induction furnace is induction heated, and the maximum temperature in the induction furnace is set to 2500°C.

[0032] The silicon raw material in the reaction precursor melts and evaporates in a high-temperature environment. The melted and evaporated silicon melt and gas react with the high-purity carbon raw material to generate silicon carbide. The induction furnace is in a vacuum hydrogen protection state. The heat source generator in the high-temperature environment of the melted and evaporated silicon raw material is heated by an induction coil.

[0033] At the same time, the preparation method of silicon carbide is realized by an electric induction furnace preparation device. In the furnace body protected by inert gas argon, the silicon raw material for producing silicon carbide is melted or evaporated in a high temperature environment exceeding 2000°C, and the melted or evaporated silicon raw material reacts with the carbon raw material to generate silicon carbide. The specific steps are as follows:

[0034] S1. Add high-purity carbon source and high-purity silicon source into a mixing device according to a certain configuration ratio. The mass ratio of high-purity carbon source to high-purity silicon source is 3:6. The three-dimensional mixing device is used for homogenization treatment to mix a uniform reaction precursor. The high-purity carbon source is one or a mixture of high-purity carbon powder, graphite or a mixture of the two. As long as the carbon contained in the carbon-containing component is sufficient to carbonize the silicon raw material, the high-purity silicon source is one or a mixture of high-purity silicon, quartz sand or a mixture of the two.

[0035] S2. After completing step S1., the reaction precursor is loaded into the graphite crucible, and the furnace protective door is fixedly locked.

[0036] S3. After completing step S2, set the parameters of the preparation device: connect the inert gas hydrogen source to the gas duct inlet, and maintain the hydrogen flow rate of the reactor at 5 to 20 L / min, which is set to 10 L / min in this embodiment.

[0037] S4. After completing step S3, open the vacuum device according to the startup operating procedures of the preparation device to maintain the vacuum degree at ≤1Pa; start the induction heating device and increase the temperature to 2200℃ according to the specified temperature curve; in order to further improve the purity and prevent secondary pollution, polish or add a coating on the inside of the furnace body, the coating is a boron carbide coating, and the flow rate of the protective gas is set within the specified range.

[0038] In this embodiment: the silicon raw material in the reaction precursor is melted and evaporated in a high-temperature environment, and the melted and evaporated silicon melt and gas react with the high-purity carbon raw material to generate silicon carbide. The induction furnace is in a vacuum hydrogen protection state, and the heat source generator in the high-temperature environment of the melted and evaporated silicon raw material is heated by an induction coil. At the same time, the silicon carbide preparation method is implemented by an electric induction furnace preparation device. In the furnace body protected by inert gas argon, the silicon raw material for producing silicon carbide is melted or evaporated in a high-temperature environment exceeding 2000°C, and the melted or evaporated silicon raw material reacts with the carbon raw material to generate silicon carbide. The silicon raw material in the high-temperature environment melts or evaporates, and reacts with the carbon raw material to generate silicon carbide. This method can efficiently prepare high-purity silicon carbide.

[0039] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0040] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing semiconductor silicon carbide ceramic material, characterized in that: The steps include: S1. Use the furnace body under the protection of hydrogen gas in a vacuum environment; S2. Using high-purity carbon source particles and high-purity silicon particles to fully mix to prepare a reaction precursor in a certain ratio; S3. According to step S2, the silicon raw material in the reaction precursor is melted and evaporated in a high temperature environment; S4. According to step S3, the melted and evaporated silicon melt reacts with the high-purity carbon raw material to generate silicon carbide.

2. The method for preparing semiconductor silicon carbide ceramic material according to claim 1, characterized in that: The particles of the high-purity carbon source and the particles of the high-purity silicon source are fully mixed to prepare a reaction precursor in a certain ratio, wherein the carbon raw material in the reaction precursor is 2-5, and the silicon raw material in the reaction precursor is 7-10.

3. The method for preparing semiconductor silicon carbide ceramic material according to claim 2, characterized in that: The carbon-containing raw materials in the reaction precursor are high-purity carbon powder and graphite.

4. The method for preparing semiconductor silicon carbide ceramic material according to claim 3, characterized in that: The particle size of the high-purity carbon powder and graphite mixed particles is 40-100 meshes.

5. The method for preparing semiconductor silicon carbide ceramic material according to claim 4, characterized in that: The purity of the high-purity carbon powder and graphite mixed particles is higher than 99.995%.

6. The method for preparing semiconductor silicon carbide ceramic material according to claim 3, characterized in that: The high-purity silicon source is set to high-purity quartz sand and high-purity silicon powder, and the impurity content of the high-purity quartz sand and the high-purity silicon powder is less than 100 ppm.

7. The method for preparing semiconductor silicon carbide ceramic material according to claim 6, characterized in that: The particle size of the mixture of the high-purity silicon powder and the high-purity quartz sand is 100-150 meshes.

8. The method for preparing semiconductor silicon carbide ceramic material according to claim 2, characterized in that: The reaction position of the reaction precursor to generate silicon carbide is in a crucible in a high-temperature induction furnace. The crucible is a high-purity graphite crucible with boron carbide sprayed on the surface. The induction furnace is induction heated, and the maximum temperature in the induction furnace is set to 2500°C.

9. The method for preparing semiconductor silicon carbide ceramic material according to claim 8, characterized in that: The silicon raw material in the reaction precursor melts and evaporates in a high-temperature environment, and the melted and evaporated silicon melt and gas react with the high-purity carbon raw material to generate silicon carbide. The induction furnace is in a vacuum hydrogen protection state.

10. The method for preparing semiconductor silicon carbide ceramic material according to claim 2, characterized in that: The heat source generator for the high temperature environment of the silicon raw material for melting and evaporation is induction coil heating.

Citation Information

Patent Citations

  • Preparation method of silicon carbide

    CN103833035A

  • Silicon carbide and preparation method thereof, silicon carbide ceramic and semiconductor device

    CN118290159A

Cited By

  • Novel silicon carbide production process

    CN119370847A

  • A process for producing silicon carbide

    CN119370847B