Hole transport material, preparation method thereof and perovskite solar cell
By using hole transport materials with specific structures in perovskite solar cells, the shortcomings in passivation defects and tolerance of traditional materials are solved, and the photoelectric conversion efficiency and stability of the battery are improved. It is suitable for calcium in inverted structures. Titanium-based solar cells.
Patent Information
- Application Number
- CN202411013553.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Traditional small molecule hole transport materials add additives to perovskite solar cells to passivate grain boundary defects and interface defects, but affect cell stability and poor tolerance to perovskite precursor solutions, resulting in cell photoelectric conversion efficiency Restricted.
Provided is a hole transport material, including compounds of formula I, which can passivate grain boundary defects and interface defects without additives, with high HOMO energy level and hole migration through specific compound structures and preparation methods. and has good tolerance and film formation to perovskite precursor solutions, and is used to prepare hole transport layers of perovskite solar cells.
It improves the photoelectric conversion efficiency and stability of perovskite solar cells, reduces pinhole morphology defects, enhances the thermal stability and repeatability of the battery, and is suitable for the preparation of inverted perovskite solar cells.
Smart Images

Figure CN118955562A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a hole transport material and a preparation method thereof, and a perovskite solar cell. Background Art
[0002] Perovskite solar cells (PSCs) are devices that use perovskite-type organic metal halide semiconductors as light-absorbing materials to directly convert light energy into electrical energy through the photovoltaic effect. Hole transport materials are important materials for preparing perovskite solar cells, and play a decisive role in improving cell performance and achieving large-scale commercial applications.
[0003] At present, the hole transport materials in perovskite solar cells are mainly divided into three categories: inorganic hole transport materials, small molecule hole transport materials and organic polymer hole transport materials. Among them, small molecule hole transport materials have the advantages of high purity and easy solution processing, and are widely used in perovskite solar cells. According to the spatial structure, traditional small molecule hole transport materials can be divided into three categories: linear structure, spirocyclic structure and star structure. According to the different groups contained in the molecular structure, traditional small molecule hole transport materials can also be divided into dithienylpyrrole type, triphenylamine type, carbazole type, bifluorene type, thiophene type, etc. In order to consider the battery performance, additives are generally added when preparing the hole transport layer using traditional small molecule hole transport materials, but the addition of additives has an adverse effect on the stability of the battery, which restricts the development of perovskite solar cells. Summary of the invention
[0004] Based on this, the first aspect of the present application provides a hole transport material and a preparation method thereof and a perovskite solar cell. The technical solution is as follows:
[0005] A hole transport material comprising a compound of formula I:
[0006]
[0007] Wherein, L is selected from C 3-5 Alkylene;
[0008] R is selected from C 1-3 alkyl;
[0009] X is selected from O or S.
[0010] The second aspect of the present application provides a method for preparing a hole transport material, and its technical solution is as follows:
[0011] A method for preparing a hole transport material comprises the following steps:
[0012] Allowing the compound of formula I-5 to undergo a substitution reaction with the compound of formula I-6 to generate a compound of formula I-7;
[0013] Allow the compound of formula I-4 to undergo Suzuki coupling reaction with the compound of formula I-7 to generate a compound of formula I-8; hydrolyze the compound of formula I-8 to generate a compound of formula I;
[0014]
[0015]
[0016] Wherein, L is selected from C 3-5 Alkylene;
[0017] R is selected from C 1-3 alkyl;
[0018] X is selected from O or S;
[0019] Y 1 are independently selected from halogen.
[0020] The third aspect of the present application provides a perovskite solar cell, and its technical solution is as follows:
[0021] A perovskite solar cell comprises a transparent conductive electrode, a first charge transport layer, a perovskite light absorbing layer, a second charge transport layer and a metal electrode stacked in sequence; the first charge transport layer or the second charge transport layer comprises the hole transport material as described above or comprises the hole transport material prepared by the preparation method as described above.
[0022] Compared with the traditional solution, this application has the following beneficial effects:
[0023] The formula I compound of the present application has a strong interaction with the components in the perovskite light-absorbing layer, and can passivate grain boundary defects and interface defects without adding additives such as P-type dopants or interface modifiers, and the battery has high photoelectric conversion efficiency and good battery stability. At the same time, the formula I compound has a HOMO energy level that matches the perovskite and is deeper, has a good hole mobility, is conducive to the extraction and transmission of holes, is conducive to the improvement of the battery photoelectric conversion efficiency, and has high repeatability. At the same time, the decomposition temperature of the formula I compound is high, the thermal stability is good, and it can be stably present under the annealing process. At the same time, in the preparation process of inverted perovskite solar cells, the perovskite precursor solution is usually printed on the hole transport layer to form a perovskite light-absorbing layer, and the traditional small molecule hole transport material has poor tolerance to the perovskite precursor solution, resulting in the presence of pinhole morphology defects, and the battery photoelectric conversion efficiency is affected. The compound of formula I has good tolerance to the perovskite precursor solution and has good film-forming properties. At the same time, after film formation, it has good wettability with the perovskite precursor solution, which is beneficial to the crystallization and film formation of the perovskite light-absorbing layer and is beneficial to improving the photoelectric conversion efficiency of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0025] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the compound of formula II in Example 1;
[0026] Figure 2 is the hydrogen nuclear magnetic resonance spectrum of the compound of formula III in Example 2;
[0027] Figure 3 Current density-voltage curves of perovskite solar cells prepared with different hole transport materials. DETAILED DESCRIPTION
[0028] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0030] the term
[0031] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0032] "Alkyl" refers to straight-chain or branched saturated aliphatic hydrocarbon groups. 1-3 Non-limiting examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl.
[0033] For battery performance considerations, when using traditional small molecule hole transport materials to prepare hole transport layers, additives such as P-type dopants or interface modifiers are generally added to passivate grain boundary defects and interface defects. However, the addition of additives has an adverse effect on the stability of the battery, restricting the development of perovskite solar cells.
[0034] In view of this, the first aspect of the present application provides a hole transport material, including a compound of formula I:
[0035]
[0036] Wherein, L is selected from C 3-5 Alkylene;
[0037] R is selected from C 1-3 alkyl;
[0038] X is selected from O or S.
[0039] Optionally, L is -(CH 2 ) 4 -, R is -CH 3 In this case, the hole transport material includes a compound of formula II or a compound of formula III:
[0040]
[0041]
[0042] The present application introduces a methoxy or methylthio triphenylamine group into the acridine phosphate side chain, and the obtained compound of formula I has a strong interaction with the components in the perovskite light-absorbing layer, and can passivate grain boundary defects and interface defects without adding additives such as P-type dopants or interface modifiers, and the battery has high photoelectric conversion efficiency and good battery stability. At the same time, the compound of formula I has a HOMO energy level that matches the perovskite and is deeper, has a good hole mobility, is conducive to the extraction and transmission of holes, is conducive to the improvement of the battery photoelectric conversion efficiency, and has high repeatability. At the same time, the decomposition temperature of the compound of formula I is high, the thermal stability is good, and it can be stably present under the annealing process. At the same time, in the preparation process of inverted perovskite solar cells, the perovskite precursor solution is usually printed on the hole transport layer to form a perovskite light-absorbing layer, and the traditional small molecule hole transport material has poor tolerance to the perovskite precursor solution, resulting in the hole transport layer always having pinhole morphology defects, and the battery photoelectric conversion efficiency is affected. The compound of formula I has good tolerance to the perovskite precursor solution and has good film-forming properties. At the same time, after film formation, it has good wettability with the perovskite precursor solution, which is beneficial to the crystallization and film formation of the perovskite light-absorbing layer and is beneficial to improving the photoelectric conversion efficiency of the battery.
[0043] The second aspect of the present application provides a method for preparing a hole transport material, comprising the following steps:
[0044] S10, subjecting the compound of formula I-1 to a substitution reaction to generate a compound of formula I-2.
[0045] Optionally, subjecting the compound of formula I-1 to a substitution reaction comprises the following steps:
[0046] The compound of formula I-1, N-bromosuccinimide and a first solvent are mixed to cause a first substitution reaction.
[0047] Optionally, the molar ratio of the compound of formula I-1 to the N-bromosuccinimide is 1:(2-3).
[0048] Optionally, the first solvent is dichloromethane.
[0049] Optionally, the temperature of the first substitution reaction is 15°C to 40°C, and the time of the first substitution reaction is 10h to 14h.
[0050] S20, subjecting the compound of formula I-2 to a substitution reaction to generate a compound of formula I-3.
[0051] Optionally, subjecting the compound of formula I-2 to a substitution reaction comprises the following steps:
[0052] Mix the compound of formula I-2, The first catalyst and the first alkali agent undergo a second substitution reaction.
[0053] Optionally, the compound of formula I-2 and The molar ratio is 1:(40~60).
[0054] Optionally, It is 1,4-dibromobutane.
[0055] Optionally, the first catalyst is selected from tetrabutylammonium bromide.
[0056] Optionally, the molar ratio of the compound of formula I-2 to the first catalyst is 1:(0.05-0.2).
[0057] Optionally, the first alkaline agent is selected from potassium hydroxide.
[0058] Optionally, the molar ratio of the compound of formula I-2 to the first alkaline agent is 1:(7-10).
[0059] Optionally, the temperature of the second substitution reaction is 60° C. to 70° C., and the time of the second substitution reaction is 10 h to 14 h.
[0060] S30, allowing the compound of formula I-3 to undergo an esterification reaction with triethyl phosphite to generate the compound of formula I-4.
[0061] Optionally, the molar ratio of the compound of formula I-3 to the triethyl phosphite is 1:(140-160).
[0062] Optionally, the esterification reaction temperature is 150° C. to 170° C., and the reaction time is 10 h to 14 h.
[0063] S40, subjecting the compound of formula I-5 to a substitution reaction with the compound of formula I-6 to generate a compound of formula I-7.
[0064] Optionally, the compound of formula I-5 is subjected to a substitution reaction with the compound of formula I-6, comprising the following steps:
[0065] The compound of formula I-5, the compound of formula I-6, the second catalyst and the second solvent are mixed to cause a third substitution reaction.
[0066] Optionally, the molar ratio of the compound of formula I-5 to the compound of formula I-6 is 1:(1-2).
[0067] Optionally, the second catalyst is selected from n-butyl lithium.
[0068] Optionally, the molar ratio of the compound of formula I-5 to the second catalyst is 1:(0.8-1.2).
[0069] Optionally, the second solvent is selected from tetrahydrofuran.
[0070] Optionally, the reaction conditions of the third substitution reaction include: reacting at -70°C to -90°C for 0.5h to 2h, and then reacting at 15°C to 40°C for 10h to 14h.
[0071] S50, subjecting the compound of formula I-4 to Suzuki coupling reaction with the compound of formula I-7 to generate a compound of formula I-8.
[0072] Optionally, the compound of formula I-4 and the compound of formula I-7 are subjected to a Suzuki coupling reaction, comprising the following steps:
[0073] The compound of formula I-4, the compound of formula I-7, a third catalyst, a second alkaline agent and a third solvent are mixed to cause a Suzuki coupling reaction.
[0074] Optionally, the molar ratio of the compound of formula I-4 to the compound of formula I-7 is 1:(2 to 2.4).
[0075] Optionally, the third catalyst is selected from tetrakis(triphenylphosphine)palladium.
[0076] Optionally, the molar ratio of the compound of formula I-4 to the third catalyst is 1: (0.04-0.06)
[0077] Optionally, the second alkaline agent is selected from potassium carbonate.
[0078] Optionally, the molar ratio of the compound of formula I-4 to the second alkaline agent is 1:(4-7).
[0079] Optionally, the third solvent is selected from at least one of toluene, ethanol and water.
[0080] Optionally, the reaction temperature of the Suzuki coupling reaction is 80° C. to 90° C., and the reaction time is 4 h to 8 h. S60, hydrolyzing the compound of formula I-8 to generate the compound of formula I.
[0081] Optionally, hydrolyzing the compound of formula I-8 comprises the following steps:
[0082] The compound of formula I-8 is hydrolyzed using a fourth solvent and a fourth catalyst.
[0083] Optionally, the fourth catalyst is selected from trimethylsilyl bromide.
[0084] Optionally, the molar ratio of the compound of formula I-8 to the fourth catalyst is 1:(8-12). Optionally, the fourth solvent includes 1,4-dioxane, methanol and water.
[0085] Optionally, the hydrolysis time is 10 h to 14 h.
[0086]
[0087]
[0088] Among them, L, R, and X are as described above and will not be repeated here.
[0089] Y 1 and Y 3 Each is independently selected from halogen, such as Br.
[0090] Y 2 is selected from halogen, such as Br.
[0091] The preparation method has simple synthesis steps, low cost, and is suitable for industrial production. The prepared hole transport material has good thermal stability and film-forming properties, and its energy level matches that of perovskite. It can be used as an undoped hole transport material in inverted perovskite solar cells to obtain good photoelectric conversion efficiency with high repeatability.
[0092] In a third aspect, the present application provides a perovskite solar cell, comprising a transparent conductive electrode, a first charge transport layer, a perovskite light absorbing layer, a second charge transport layer and a metal electrode stacked in sequence; the first charge transport layer or the second charge transport layer comprises the hole transport material as described above or comprises a hole transport material prepared by the preparation method as described above.
[0093] Optionally, the first charge transport layer is a hole transport layer, the second charge layer is an electron transport layer, and the first charge transport layer includes the hole transport material or includes a hole transport material prepared by the preparation method. At this time, the perovskite solar cell is an inverted perovskite solar cell, and the above-mentioned hole transport layer material is particularly suitable for inverted perovskite solar cells. In the preparation process of the inverted perovskite solar cell, the perovskite precursor solution is usually printed on the hole transport layer to form a perovskite light absorption layer, and the traditional small molecule hole transport material has poor tolerance to the perovskite precursor solution, resulting in the presence of pinhole morphology defects, and the cell photoelectric conversion efficiency is affected. The compound of formula I has good tolerance to the perovskite precursor solution, and has good film-forming properties. At the same time, after film formation, it also has good wettability with the perovskite precursor solution, which is conducive to the crystallization and film formation of the perovskite light absorption layer, and is conducive to improving the cell photoelectric conversion efficiency.
[0094] In one embodiment, see Figure 1 The structure of the perovskite solar cell 100 includes a transparent conductive electrode 11, a hole transport layer 12, a perovskite absorption layer 13, an electron transport layer 14, and a metal electrode 15 stacked in sequence.
[0095] The transparent conductive electrode 11 is ITO glass.
[0096] The hole transport layer 12 includes the hole transport material as described above or includes the hole transport material prepared by the preparation method as described above. The hole transport layer 12 can be prepared by the following method: dissolving the hole transport material in a solvent to obtain a solution, coating the solution and annealing. Optionally, each 1 mL of the solution contains 3 mg to 15 mg of the hole transport material. Optionally, the solvent can be chlorobenzene, toluene, dichloromethane, etc. The above-mentioned hole transport materials have good solubility in solvents such as toluene, chlorobenzene, dichloromethane, etc. Optionally, the annealing temperature is 90 to 110°C.
[0097] The perovskite absorption layer 13 is a quasi-two-dimensional perovskite. The perovskite absorption layer 13 can be prepared by the following method: dissolving the perovskite material in a solvent to obtain a solution, coating the solution and then annealing. Optionally, the perovskite material is selected from at least one of 3-bromobenzylammonium iodide, 3-chlorobenzylammonium iodide, methylammonium chloride and lead iodide. Optionally, the solvent can be at least one of DMF and DMSO.
[0098] The electron transport layer 14 includes PC61BM.
[0099] The metal electrode is at least one of chromium (Cr) and gold (Au).
[0100] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0101] Example 1
[0102] S10, subjecting the compound of formula (1) to a substitution reaction to generate a compound of formula (2)
[0103]
[0104] In a 100 mL round bottom bottle, add the compound of formula (1) (0.89 g, 4.24 mmol) and dichloromethane (10 mL), and then add N-bromosuccinimide (1.51 g, 8.48 mmol). The mixture is heated to room temperature and then stirred overnight. The reaction is quenched with water, extracted with dichloromethane, the organic layers are combined, dried over anhydrous magnesium sulfate, and then the organic solvent is removed by rotary evaporator to obtain a crude product. Further purification is carried out by flash column chromatography with an eluent of petroleum ether / dichloromethane 10 / 1. The compound of formula (2) is obtained as a white solid (1.40 g, yield 90%)
[0105] S20, subjecting the compound of formula (2) to a substitution reaction to generate a compound of formula (3)
[0106]
[0107] In a 100mL double-necked bottle, add the compound of formula (2) (1.00g, 2.72mmol), tetrabutylammonium bromide (0.32g, 0.27mmol) dissolved in 1,4-dibromobutane (15mL, 125mmol), and then dropwise add 50wt% potassium hydroxide aqueous solution (5mL). The mixture is heated to 65°C and then stirred overnight. The reaction is quenched with water, extracted with dichloromethane, the organic layer is combined with anhydrous magnesium sulfate and dried, and then the organic solvent is removed by a rotary evaporator to obtain a crude product. Further purification is performed by silica gel column chromatography with an eluent of petroleum ether / dichloromethane = 10 / 1 to obtain the compound of formula (3) as a colorless oil (1.20g, yield 89%).
[0108] S30, allowing the compound of formula (3) to undergo an esterification reaction with triethyl phosphite to generate the compound of formula (4)
[0109]
[0110] In a 100 mL double-necked flask, add the compound of formula (3) (1.20 g, 2.39 mmol) and triethyl phosphite (10 mL), then heat the mixture to 160° C. and stir overnight under a nitrogen atmosphere. Then remove the organic solvent with a rotary evaporator to obtain a crude product of the compound of formula (4) (1.30 g, 2.27 mmol)
[0111] S40, causing the compound of formula (5) to undergo a substitution reaction with the compound of formula (6) to generate a compound of formula (7)
[0112]
[0113] Weigh the compound of formula (5) (3.84 g, 10 mmol) into a 500 mL three-necked flask, then add 30 mL of dry THF and heat under N 2 The mixture was cooled to -78°C and stirred for 10 min, then n-butyl lithium (3.75 mL, 1.00 equiv, 1.6 Min n-hexane) was slowly added dropwise, and the mixture was reacted at -78°C for 1 hour. Then, the compound of formula (6) (2.75 mL, 15 mmol) was added, and the reaction was continued at -78°C for 1 hour, and finally the mixture was moved to room temperature for 12 hours. The reaction was quenched with 50 mL of deionized water, extracted with saturated NaCl solution and DCM, and the organic phase was anhydrous MgSO4. 2 SO 4 The product was dried, filtered, and finally purified by column chromatography (PE:DCM=15:1) to obtain 3.4 g of a white solid compound of formula (7) with a yield of 79%.
[0114] S50, subjecting the compound of formula (4) to Suzuki coupling reaction with the compound of formula (7) to generate a compound of formula (8)
[0115]
[0116] In a 100 mL double-necked flask, the compound of formula (4) (0.58 g, 1 mmol), the compound of formula (7) (0.9 g, 2.2 mmol), tetrakis(triphenylphosphine)palladium (57 mg, 0.05 mmol), and potassium carbonate (0.83 g, 6 mmol) were added. The solvent was toluene, ethanol, and water (ratio 2:1:1). The reaction was carried out at 85°C for 6 hours. The mixture was cooled to room temperature, extracted with DCM, and anhydrous Mg was added. 2 SO 4 The organic phase was dried, filtered, and distilled under reduced pressure, and finally purified by column chromatography (PE:DCM=4:1) to obtain the compound of formula (8) (0.75 g, 0.74 mmol) with a yield of 75%.
[0117] S60, hydrolyzing the compound of formula (8) to generate a compound of formula II
[0118]
[0119] In a 100mL double-necked flask, add the compound of formula (8) (2.04g, 2mmol) to anhydrous 1,4-dioxane (10mL) at room temperature, add trimethylsilyl bromide (3.06g, 20mmol), and then stir overnight. Remove 1,4-dioxane with a rotary evaporator to obtain a solid powder. Dissolve the solid powder in methanol (10mL) at room temperature, then add deionized water dropwise until the mixture becomes opaque, and stir for another 12 hours. The crude product is collected by filtration and washed with deionized water. The crude product is dissolved in THF (5mL), reprecipitated in acetone (20mL), and filtered to obtain the final product, which is a compound of formula II (1.2g, yield 75%). The hydrogen nuclear magnetic resonance spectrum of the compound of formula II is shown as follows Figure 1 shown.
[0120] Example 2
[0121] S10 to S30 refer to Example 1.
[0122] S40, subjecting the compound of formula (9) to a substitution reaction with the compound of formula (6) to generate a compound of formula (10)
[0123]
[0124] Weigh the compound of formula (5) (4.17 g, 10 mmol) into a 500 mL three-necked flask, then add 30 mL of dry THF and heat under N 2 The mixture was cooled to -78°C and stirred for 10 min, then n-butyl lithium (3.75 mL, 1.00 equiv, 1.6 Min n-hexane) was slowly added dropwise, and the mixture was reacted at -78°C for 1 hour. Then, the compound of formula (6) (2.75 mL, 15 mmol) was added, and the reaction was continued at -78°C for 1 hour, and finally the mixture was moved to room temperature for 12 hours. The reaction was quenched with 50 mL of deionized water, extracted with saturated NaCl solution and DCM, and the organic phase was anhydrous MgSO4. 2 SO 4 The product was dried, filtered, and finally purified by column chromatography (PE:DCM=15:1) to obtain 3.3 g of a white solid compound of formula (7) with a yield of 78%.
[0125] S50, subjecting the compound of formula (4) to Suzuki coupling reaction with the compound of formula (10) to generate a compound of formula (11)
[0126]
[0127] In a 100 mL double-necked flask, add the compound of formula (4) (0.58 g, 1 mmol), the compound of formula (10) (1.02 g, 2.2 mmol), tetrakis(triphenylphosphine)palladium (57 mg, 0.05 mmol), potassium carbonate (0.83 g, 6 mmol), and the solvent is toluene, ethanol and water (ratio 2:1:1), and react at 85°C for 6 hours. Cool to room temperature, extract the mixture with DCM, and add anhydrous MgSO4. 2 SO 4 The organic phase was dried, filtered, and distilled under reduced pressure, and finally purified by column chromatography (PE:DCM=4:1) to obtain the compound of formula (11) (0.78 g, 0.72 mmol) with a yield of 72%.
[0128] S60, hydrolyzing the compound of formula (10) to generate a compound of formula III
[0129]
[0130] In a 100mL double-necked flask, add the compound of formula (11) (2.17g, 2mmol) to anhydrous 1,4-dioxane (10mL) at room temperature, add trimethylsilyl bromide (3.06g, 20mmol), and then stir overnight. Remove 1,4-dioxane with a rotary evaporator to obtain a solid powder. Dissolve the solid powder in methanol (10mL) at room temperature, then add deionized water dropwise until the mixture becomes opaque, and stir for another 12 hours. The crude product is collected by filtration and washed with deionized water. The crude product is dissolved in THF (5mL), reprecipitated in acetone (20mL), and filtered to obtain the final product, which is a compound of formula III (1.3g, yield 75%). The hydrogen nuclear magnetic resonance spectrum of the compound of formula II is shown as follows Figure 2 shown.
[0131] Example 3
[0132] The compound of formula II prepared in Example 1 and the compound of formula III prepared in Example 2 were used as hole transport materials to prepare a perovskite solar cell, and the steps were as follows:
[0133] (1) Cleaning: The ITO glass sheet was ultrasonically cleaned with deionized water, acetone, and ethanol for 15 minutes, and then with N 2 The residual solvent on the surface of the ITO glass sheet was blown dry with an air gun, and then oxygen plasma treatment was performed for 15 minutes, and then the ITO glass sheet was transferred to a nitrogen glove box.
[0134] (2) Preparation of hole transport layer: 10 mg of the compound of formula II or III was weighed and completely dissolved in 1 mL of chlorobenzene solution, and an appropriate amount of the solution was evenly added dropwise onto the ITO glass substrate, spin-coated at 5000 rpm for 20 seconds, and then annealed at 100° C. for 10 minutes;
[0135] (3) Preparation of perovskite absorption layer: The ITO / hole transport layer substrate obtained above was cooled to room temperature, preheated at 130°C for 5 minutes, 50 μL of perovskite solution was spread over the ITO / hole transport layer substrate, spin-coated at 5000 rpm for 20 seconds, and then annealed at 100°C for 10 minutes to prepare a perovskite absorption layer. The perovskite solution is a DMSO solution of 3-bromobenzylammonium iodide;
[0136] (4) Preparation of electron transport layer: The ITO / hole transport layer / perovskite substrate obtained above was cooled to room temperature, PC61BM was prepared into a 15 mg / mL solution, and then 40 μL of the PC61BM solution was spread over the ITO / hole transport layer / perovskite substrate, and spin-coated at 1000 rpm for 30 to 50 seconds;
[0137] (5) Preparation of electrodes: The above substrate is placed in a vacuum evaporation chamber, and Cr (6 nm) and Au (80 nm) are evaporated on the PC61BM layer respectively, thereby obtaining the desired inverted perovskite solar cell.
[0138] Comparative Example
[0139] Using PTAA as the hole transport material, an inverted perovskite solar cell was prepared according to the method of Example 3.
[0140] Test items
[0141] Adjust the solar simulator power to 100mw / cm 2 To simulate the AM1.5G radiation standard, the current and voltage values of the device are read by a computer connected to a Keithley2450 power meter. Before measuring the current density-voltage curve, the light intensity is calibrated using a Newport standard silicon cell 91150. The device adopts forward and reverse scanning mode with a scanning rate of 0.05V / s. The current density-voltage curve after the test is shown in Figure 1 , open circuit voltage V oc , short circuit current J sc , fill factor FF and photoelectric conversion efficiency PCE are shown in Table 1.
[0142] Table 1
[0143]
[0144] It can be seen that the open circuit voltage of the inverted perovskite solar cell device corresponding to PTAA, which is currently commonly used in inverted devices, is 1.19V and the short circuit current is 20.72mA / cm 2 , the filling factor is 75.01%, and the photoelectric conversion efficiency is 18.51%.
[0145] The open circuit voltage of the inverted perovskite solar cell device corresponding to the compound of formula II is 1.15V and the short circuit current is 20.46mA / cm 2 , the filling factor is 79.88%, and the photoelectric conversion efficiency is 18.89%.
[0146] The inverted perovskite solar cell device corresponding to the compound of formula III has an open circuit voltage of 1.16 V and a short circuit current of 20.47 mA / cm 2 , the filling factor is 80.74%, and the photoelectric conversion efficiency is 19.23%.
[0147] It can be seen that the perovskite solar cell based on the undoped hole transport material of the compound of formula II or the compound of formula III can obtain good device performance.
[0148] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0149] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A hole transport material, characterized in that: Includes compounds of formula I: Wherein, L is selected from C 3-5 Alkylene; R is selected from C 1-3 alkyl; X is selected from O or S.
2. The hole transport material according to claim 1, characterized in that L is -(CH2)4-, and R is -CH3.
3. A method for preparing a hole transport material, characterized in that: The following steps are involved: Allowing the compound of formula I-5 to undergo a substitution reaction with the compound of formula I-6 to generate a compound of formula I-7; Allow the compound of formula I-4 to undergo Suzuki coupling reaction with the compound of formula I-7 to generate a compound of formula I-8; hydrolyze the compound of formula I-8 to generate a compound of formula I; Wherein, L is selected from C 3-5 Alkylene; R is selected from C 1-3 alkyl; X is selected from O or S; Y1 and Y3 are each independently selected from halogen.
4. The method for preparing a hole transport material according to claim 3, characterized in that: The compound of formula I-5 and the compound of formula I-6 undergo a substitution reaction, comprising the following steps: The compound of formula I-5, the compound of formula I-6, the second catalyst and the second solvent are mixed to cause a third substitution reaction.
5. The method for preparing a hole transport material according to claim 3, characterized in that: The compound of formula I-4 and the compound of formula I-7 undergo Suzuki coupling reaction, comprising the following steps: The compound of formula I-4, the compound of formula I-7, a third catalyst, a second alkaline agent and a third solvent are mixed to cause a Suzuki coupling reaction.
6. The method for preparing a hole transport material according to claim 3, characterized in that: The method of hydrolyzing the compound of formula I-8 comprises the following steps: The compound of formula I-8 is hydrolyzed using a fourth solvent and a fourth catalyst.
7. The method for preparing a hole transport material according to any one of claims 3 to 6, characterized in that: The preparation method of the compound of formula I-4 comprises the following steps: Substituting the compound of formula I-1 to generate a compound of formula I-2; Allowing the compound of formula I-2 to undergo a substitution reaction to generate a compound of formula I-3; Allowing the compound of formula I-3 to undergo an esterification reaction with triethyl phosphite to generate the compound of formula I-4; Wherein, Y2 is selected from halogen.
8. The method for preparing a hole transport material according to claim 7, characterized in that: The compound of formula I-1 is subjected to a substitution reaction, comprising the following steps: The compound of formula I-1, N-bromosuccinimide and a first solvent are mixed to cause a first substitution reaction.
9. The method for preparing a hole transport material according to claim 7, characterized in that: The compound of formula I-2 is subjected to a substitution reaction, comprising the following steps: Mix the compound of formula I-2, The first catalyst and the first alkali agent undergo a second substitution reaction.
10. A perovskite solar cell, characterized in that: It comprises a transparent conductive electrode, a first charge transport layer, a perovskite light absorbing layer, a second charge transport layer and a metal electrode stacked in sequence; the first charge transport layer or the second charge transport layer comprises the hole transport material according to any one of claims 1 to 2 or comprises the hole transport material prepared by the preparation method according to any one of claims 3 to 9.
Citation Information
Patent Citations
Self-assembly hole selection material based on acridine and preparation method and application thereof
CN116178430A
Spiro organic compound and application thereof in organic electronic device
CN117447515A
Acridone compound as well as preparation method and application thereof
CN117924366A
Self-assembled hole transport material and preparation method and application thereof
CN118206586A
Inversion wide-band-gap perovskite solar cell and preparation method thereof
CN118251022A
Cited By
Hole transport material, preparation method thereof and perovskite solar cell
CN119504859A
Organic compound and preparation method thereof, hole transport material and solar cell
CN120398861A
Perovskite solar cell, laminated cell and photovoltaic module
CN121531887A
Self-assembling molecule, perovskite solar cell, photovoltaic module, power generation device, and electric device
WO2026067617A1