Alkene acid ester crown ether polymer as well as synthesis method and application thereof
By developing the enoic acid ether polymer, the problem of dissolution of small crown ether molecules during the circulation process is solved, and the efficient extraction of lithium ions in the salt lake brine is achieved, which significantly improves the adsorption capacity and selective separation capacity, and improves the material Stability and environmental adaptability.
Patent Information
- Application Number
- CN202411042406.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The existing small crown ether organic molecules dissolve during circulation, resulting in a degradation of adsorbent performance and inability to effectively extract lithium ions in salt lake brine.
Develop a new lithium adsorption material based on enoate crown ether polymers, prepare enoate crown ether monomers through esterification reactions, and obtain polymer materials through free radical polymerization to improve the rigidity of the material and lithium ion capture ability.
It significantly improves the adsorption capacity and selective separation ability of lithium ions, improves the mechanical and thermal properties of the materials, has good stability, and adapts to environmental needs.
Smart Images

Figure CN118955774A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an acrylate crown ether polymer and a synthesis method and application thereof, belonging to the technical field of polymer materials. Background Art
[0002] Salt lake brine has the characteristics of high salt concentration, high magnesium-lithium ratio and complex composition, and the separation of lithium in brine is challenging. At present, the main technologies for extracting lithium from salt lake brine include adsorption, membrane, chemical precipitation, extraction, crystallization, flotation and ion distillation. The adsorption method is considered to be one of the most promising technologies for directly extracting lithium from salt lake brine (especially low-grade, high magnesium-lithium ratio brine) because of its advantages such as low requirements for brine pretreatment, high lithium selectivity and recovery rate, additional concentration function, cost-effectiveness and environmental friendliness.
[0003] Salt lake brine resources are located in the plateau, with inconvenient transportation and backward industrial infrastructure. In view of the current fragile ecosystem and environmental protection issues in the plateau, the adsorption method (mobile vehicle adsorption, electrosorption) has certain advantages. It is an energy-saving, green, environmentally friendly, simple to operate and efficient separation technology.
[0004] The core of the adsorption method lies in the adsorption material. Existing lithium adsorption materials mainly include inorganic adsorption materials and organic adsorption materials. Common inorganic adsorption materials include lithium aluminum layered double hydroxide, lithium titanium oxide type lithium ion sieve, and lithium manganese oxide type lithium ion sieve. The basic principle is that the inorganic ion sieve introduces lithium ions into it through exchange, and then elutes them from the crystal structure of aluminum hydroxide or manganese and titanium oxides to produce lithium ion-specific vacancies, and uses the crystal memory effect to achieve selective lithium extraction. Organic adsorption materials include ion-imprinted polymers and ion exchange resins. Macrocyclic compounds such as crown ethers have attracted much attention because they can selectively bind lithium ions.
[0005] Crown ethers are cyclic compounds formed by ether bonds. They can react with metal ions through the electrostatic effect of dipole charges to form stable complexes. Their organic small molecules are often used for selective extraction of metal ions, and their organic polymers are often doped into adsorbents or nanofiltration membranes for adsorption and filtration.
[0006] Chinese patent CN202410185109.0 uses nitrobenz-12-crown-4 to obtain aminobenzo-12-crown-4 by nucleophilic substitution with hydrazine hydrate, and then dopes it into a resin to obtain a resin-based material grafted with a crown ether group. The new resin-based adsorbent material is measured by the lithium ion adsorption determination method described in the patent, and the lithium adsorption capacity reaches up to 13.76 mg / g.
[0007] Chinese patent CN202410058182.1 uses 12-crown ether-4, polyvinyl chloride, and lithium salt to add to an organic solvent, blend and dry to obtain a lithium ion specific adsorbent. The material was tested for lithium ion adsorption, and its maximum lithium adsorption capacity was 3.58 mg / g.
[0008] The above patents have pioneered a series of crown ether-based organic molecule modifications and achieved significant results in lithium ion adsorption, but these patents have ignored a common problem, that is, trying to forcibly blend organic small molecules with matrix materials, and especially crown ether organic small molecules, because the carbon ring organic components account for more than 80%, and there are no water-soluble groups such as hydroxyl carboxyl groups, which will cause the crown ether small molecules to be unable to couple with the blended matrix and brine. The crown ether small molecules slowly dissolve during the cycle, and ultimately manifest as a serious decrease in the performance of the adsorbent during the cycle. Therefore, based on these works, changing the direction of small molecule research and development to develop new organic lithium ion sieve adsorbents based on crown ether polymers is a basic requirement for adapting to the development of salt lake lithium extraction technology. Summary of the invention
[0009] In view of the shortcomings of the prior art, the object of the present invention is to provide a new lithium adsorption material based on crown ether segment polymer.
[0010] Another object of the present invention is to provide a method for synthesizing the novel lithium adsorption material of the present invention.
[0011] Another object of the present invention is to apply the novel lithium adsorption material of the present invention to separate and enrich lithium ions in salt lake brine.
[0012] To achieve the above object, the present invention provides an acrylate crown ether polymer, which is composed of the following repeating structural units: acrylate crown ether, and has a number average molecular weight of 6700 to 15000.
[0013]
[0014] Wherein, m is the number of repetitions of ethoxy groups in the enoate crown ether ring, n is the number of repetitions of the enoate crown ether, and R1 and R2 are linking groups on the enoate crown ether.
[0015] The repetition number m of the ethoxy group in the acrylate crown ether ring includes m=1, 2 and 3, that is, the acrylate crown ether includes acrylate 12 crown 4, acrylate 15 crown 5 and acrylate 18 crown 6. Preferably, the repetition number m of the ethoxy group in the acrylate crown ether ring is 1, that is, the acrylate crown ether is acrylate 12 crown 4, and the diameter of its crown ether ring cavity is equivalent to the diameter of lithium ions. In addition, due to the strengthening effect of the ester group, it has specific adaptability to lithium ions and significantly improves its selective separation ability.
[0016] The connecting group R1 on the acrylate crown ether includes CH3-, F, and H, and R2 includes CH3- and H, preferably R1 = CH3- or F, or R2 = CH3-, that is, the acrylate in the acrylate crown ether is an acrylate derivative with rigid groups such as methyl, fluoride ion, etc. The rigid groups are connected to the main chain of the acrylate crown ether polymer, which significantly improves the rigidity of the main chain, thereby improving the ability of the acrylate crown ether polymer to capture lithium ions.
[0017] The synthesis method of the above-mentioned acrylate crown ether polymer comprises the following steps:
[0018] A. preparing an acrylate crown ether monomer, comprising:
[0019] (A1) weighing 2-hydroxymethyl-crown ether and an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:1 to 4;
[0020] (A2) adding 1 to 2 times the amount of 2-hydroxymethyl-crown ether substance as esterification aid and mixing evenly;
[0021] (A3) adding 1 to 1.5 times the amount of 2-hydroxymethyl-crown ether substance in an amount of acyl chloride derivative to carry out esterification reaction at 0°C to 20°C for 1 hour to 2 hours;
[0022] (A4) After the reaction is completed, the product is separated and purified by column chromatography, the column chromatography material is selected from 100-300 mesh chromatography silica gel, the eluent is selected from a mixture of petroleum ether and ethyl acetate, the chromatography separation and purification is performed, and the eluent of the purified product is collected and distilled under reduced pressure to obtain an ester crown ether monomer, the chemical structure of which is:
[0023]
[0024] Wherein, m is the number of repetitions of ethoxy groups in the enoate crown ether ring, and R1 and R2 are connecting groups on the enoate crown ether.
[0025] B Preparation of acrylate crown ether polymers
[0026] (B1) weighing the acrylate crown ether monomer prepared in step A and mixing it with an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:0.5 to 1;
[0027] (B2) adding 1% to 10% of a free radical polymerization initiator in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution at 40° C. to 70° C. for 6 h to 24 h;
[0028] (B3) After the reaction is completed, the solid precipitate is distilled under reduced pressure to obtain a solid precipitate, which is washed with the corresponding anhydrous organic solvent in step B1 for more than 3 times and dried to obtain the enoate crown ether polymer.
[0029] Generally, the anhydrous organic solvent includes methanol, ethanol, dichloromethane, chloroform, tetrahydrofuran, N,N-dimethylformamide or a mixture thereof, which can be prepared by redistillation or dehydration with molecular sieves.
[0030] The 2-hydroxymethyl-crown ether in step A includes 2-hydroxymethyl-12-crown-4, 2-hydroxymethyl-15-crown-5 and 2-hydroxymethyl-18-crown-6, and its general chemical structure is:
[0031]
[0032] Here, m is the number of repetitions of the ethoxy group in the crown ether ring.
[0033] The esterification auxiliary agent in step A includes sodium carbonate, sodium hydroxide, ammonia water and triethylamine.
[0034] The acyl chloride derivatives in step A include acryloyl chloride, crotonyl chloride, 2-fluoroacryloyl chloride and methacryloyl chloride, and their general chemical structures are as follows:
[0035]
[0036] Among them, R1 includes CH3-, F, and H, and R2 includes CH3- and H.
[0037] The mixed solution of petroleum ether and ethyl acetate in step A includes a mixed solution with a volume ratio of 1-2:1-2.
[0038] The free radical polymerization initiator in step B includes potassium persulfate, azobisisobutyronitrile and diisopropylbenzene peroxide.
[0039] The above-mentioned acrylate crown ether polymer can be used to separate and enrich lithium ions in salt lake brine.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] 1. The adsorption capacity of the enoate crown ether polymer of the present invention for lithium ions can reach 36.07 mg / g, which has obvious advantages over the existing lithium extraction adsorbents. The enoate crown ether polymer of the present invention is based on a crown ether segment polymer, which is directly polymerized from a crown ether derivative body. The crown ether functional group has a large density, many adsorption sites, and a large adsorption capacity for lithium ions. On the other hand, the main chain of the enoate crown ether polymer uses a rigid connecting group, which improves the rigidity of the main chain, thereby improving the ability of the enoate crown ether polymer to capture lithium ions.
[0042] 2. The acrylate crown ether polymer of the present invention preferably has an acrylate crown ether derivative monomer of acrylate-12-crown-4 monomer, whose crown ether ring cavity diameter is comparable to that of lithium ions, and has a strengthening effect of the ester group, has a specific adaptability to lithium ions, and improves its selective separation ability.
[0043] 3. The enoate crown ether polymer of the present invention is a crown ether derivative bulk polymer, and its mechanical and thermal properties are greatly improved, and it has good stability and strong adaptability to the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is the chemical formula of acrylate crown ether polymer.
[0045] Figure 2 Poly(12-crown-4)-2-methacrylate NMR 1 H spectrum.
[0046] Figure 3 Poly(12-crown-4)-2-methacrylate NMR 13 C spectrum. DETAILED DESCRIPTION
[0047] To enable those skilled in the art to implement the present invention, the present invention is described in detail below. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0048] The present invention provides an acrylate crown ether polymer, such as Figure 1 As shown in the figure, it is composed of repeating structural units of acrylate crown ether, m is the number of repetitions of ethoxy groups in the acrylate crown ether ring, n is the number of repetitions of acrylate crown ether, and R1 and R2 are connecting groups on the acrylate crown ether.
[0049] The repetition number m of the ethoxy group in the crown ether ring includes m=1, 2 and 3, that is, the acrylate crown ether includes acrylate 12 crown 4, acrylate 15 crown 5 and acrylate 18 crown 6. Preferably, the repetition number m of the ethoxy group in the acrylate crown ether ring is 1, that is, the acrylate crown ether is acrylate 12 crown 4, and the diameter of its crown ether ring cavity is equivalent to the diameter of lithium ions. In addition, due to the strengthening effect of the ester group, it has specific adaptability to lithium ions and significantly improves its selective separation ability.
[0050] The connecting group R1 on the acrylate crown ether includes CH3-, F, and H, and R2 includes CH3- and H, preferably R1 = CH3- or F, or R2 = CH3-, that is, the acrylate in the acrylate crown ether is an acrylate derivative with rigid groups such as methyl, fluoride ion, etc. The rigid groups are connected to the main chain of the acrylate crown ether polymer, which significantly improves the rigidity of the main chain, thereby improving the ability of the acrylate crown ether polymer to capture lithium ions.
[0051] Figure 2 Poly(12-crown-4)-2-methacrylate NMR 1 H spectrum.
[0052] Figure 3Poly(12-crown-4)-2-methacrylate NMR 13 C spectrum.
[0053] The synthesis method of the above-mentioned acrylate crown ether polymer comprises the following steps:
[0054] A. preparing an acrylate crown ether monomer, comprising:
[0055] (A1) weighing 2-hydroxymethyl-crown ether and an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:1 to 4;
[0056] (A2) adding 1 to 2 times the amount of 2-hydroxymethyl-crown ether substance as esterification aid and mixing evenly;
[0057] (A3) adding 1 to 1.5 times the amount of 2-hydroxymethyl-crown ether substance in an amount of acyl chloride derivative to carry out esterification reaction at 0°C to 20°C for 1 hour to 2 hours;
[0058] (A4) After the reaction is completed, the product is separated and purified by column chromatography, the column chromatography material is selected from 100-300 mesh chromatography silica gel, the eluent is selected from a mixture of petroleum ether and ethyl acetate, the chromatography separation and purification is performed, and the eluent of the purified product is collected and distilled under reduced pressure to obtain an ester crown ether monomer, the chemical structure of which is:
[0059]
[0060] Wherein, m is the number of repetitions of ethoxy groups in the enoate crown ether ring, and R1 and R2 are connecting groups on the enoate crown ether.
[0061] B Preparation of acrylate crown ether polymers
[0062] (B1) weighing the acrylate crown ether monomer prepared in step A and mixing it with an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:0.5 to 1;
[0063] (B2) adding 1% to 10% of a free radical polymerization initiator in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution at 40° C. to 70° C. for 6 h to 24 h;
[0064] (B3) After the reaction is completed, the solid precipitate is distilled under reduced pressure to obtain a solid precipitate, which is washed with the corresponding anhydrous organic solvent in step B1 for more than 3 times and dried to obtain the enoate crown ether polymer.
[0065] Generally, the anhydrous organic solvent includes methanol, ethanol, dichloromethane, chloroform, tetrahydrofuran, N,N-dimethylformamide or a mixture thereof, which can be prepared by redistillation or dehydration with molecular sieves.
[0066] The 2-hydroxymethyl-crown ether in step A includes 2-hydroxymethyl-12-crown 4, 2-hydroxymethyl-15-crown 5 and 2-hydroxymethyl-18-crown 6, and its general chemical structure is:
[0067]
[0068] Here, m is the number of repetitions of the ethoxy group in the crown ether ring.
[0069] The esterification auxiliary agent in step A includes sodium carbonate, sodium hydroxide, ammonia water and triethylamine.
[0070] The acyl chloride derivatives in step A include acryloyl chloride, crotonyl chloride, 2-fluoroacryloyl chloride and methacryloyl chloride, and their general chemical structures are as follows:
[0071]
[0072] Among them, R1 includes CH3-, F, and H, and R2 includes CH3- and H.
[0073] The mixed solution of petroleum ether and ethyl acetate in step A includes a mixed solution with a volume ratio of 1-2:1-2.
[0074] The free radical polymerization initiator in step B includes potassium persulfate, azobisisobutyronitrile and diisopropylbenzene peroxide.
[0075] The following are some examples of the synthesis of acrylate crown ether polymers.
[0076]
Example 1
[0077] First, prepare an ester crown ether monomer, weigh 0.2 mol of 2-hydroxymethyl-18-crown-6 and a mixed solvent of anhydrous ethanol and anhydrous methanol in a volume ratio of 1:1 to prepare a mixed solution with a molar ratio of 1:2; add 0.26 mol of sodium carbonate and mix evenly; drop 0.2 mol of acryloyl chloride to carry out esterification reaction, and react at 20°C for 2 hours; after the reaction, separate and purify the product by chromatographic column chromatography, the column chromatography material is 100-200 mesh chromatography silica gel, the eluent is a mixed solution of petroleum ether and ethyl acetate in a volume ratio of 2:1, chromatographic separation and purification, collect the purified product eluent and distill under reduced pressure to obtain 18-crown-6-2-methyl acrylate.
[0078] Then, an ester crown polymer was prepared, and 0.1 mol of the prepared 18-crown-6-2-methyl acrylate was weighed and mixed with anhydrous N,N-dimethylformamide to prepare a mixed solution with a molar ratio of 1:1; 0.005 mol of potassium persulfate was added in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution, and the reaction was carried out at 50°C for 10 hours; after the reaction was completed, the solid precipitate was distilled under reduced pressure to obtain a solid precipitate, which was repeatedly washed with the corresponding anhydrous N,N-dimethylformamide, and freeze-dried to obtain poly-18-crown-6-2-methyl acrylate. The number average molecular weight (Mn) of the obtained poly-18-crown-6-2-methyl acrylate was 15,000 for analysis by gel permeation chromatography (GPC).
[0079]
Example 2
[0080] First, prepare an ester crown ether monomer, weigh 0.2 mol of 2-hydroxymethyl-18-crown-6 and anhydrous dichloromethane to prepare a mixed solution with a molar ratio of 1:4; add 0.3 mol of triethylamine and mix well; add 0.3 mol of acryloyl chloride dropwise for esterification reaction, and react at 0°C for 3 hours; after the reaction, separate and purify the product by column chromatography, the column chromatography material is 200-300 mesh chromatography silica gel, the eluent is a mixture of petroleum ether and ethyl acetate in a volume ratio of 1:1, perform chromatography separation and purification, collect the purified product eluent and distill under reduced pressure to obtain 18-crown-6-2-methyl acrylate.
[0081] Then, an acrylate crown polymer was prepared, and 0.1 mol of the prepared 18-crown-6-2-methyl acrylate was weighed and mixed with anhydrous tetrahydrofuran to prepare a mixed solution with a molar ratio of 1:1; 0.005 mol of potassium persulfate was added in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution, and the reaction was carried out at 50°C for 10 hours; after the reaction was completed, the solid precipitate was distilled under reduced pressure to obtain a solid precipitate, which was repeatedly washed with the corresponding anhydrous tetrahydrofuran, and freeze-dried to obtain poly-18-crown-6-2-methyl acrylate. The number average molecular weight (Mn) of the obtained poly-18-crown-6-2-methyl acrylate was 13,000 for analysis by gel permeation chromatography (GPC).
[0082]
Example 3
[0083] First, prepare an ester crown ether monomer, weigh 0.2 mol of 2-hydroxymethyl-12-crown-4 and a mixed solvent of anhydrous ethanol and anhydrous methanol in a volume ratio of 1:1 to prepare a mixed solution with a molar ratio of 1:1; add 0.3 mol of sodium hydroxide and mix evenly; dropwise add 0.25 mol of crotonyl chloride to carry out esterification reaction, and react at 40°C for 1 hour; after the reaction, separate and purify the product by chromatographic column chromatography, the column chromatography material is 100-200 mesh chromatography silica gel, the eluent is a mixed solution of petroleum ether and ethyl acetate in a volume ratio of 2:1, perform chromatography separation and purification, collect the purified product eluent and distill under reduced pressure to obtain 12-crown-4-2-butenoic acid methyl ester.
[0084] Then, an ester crown ether polymer is prepared, 0.1 mol of the prepared 12-crown ether-4-2-butenoic acid methyl ester is weighed and mixed with anhydrous dichloromethane to prepare a mixed solution with a molar ratio of 1:1; 0.01 mol of azobisisobutyronitrile is added in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution, and the reaction is carried out at 40°C for 24 hours; after the reaction is completed, the solid precipitate is distilled under reduced pressure to obtain a solid precipitate, which is repeatedly washed with the corresponding anhydrous dichloromethane and freeze-dried to obtain poly-12-crown ether-4-2-butenoic acid methyl ester. The number average molecular weight (Mn) of the obtained poly-12-crown ether-4-2-butenoic acid methyl ester is 6700 for analysis by gel permeation chromatography (GPC).
[0085]
Example 4
[0086] First, prepare an ester crown ether monomer, weigh 0.2 mol of 2-hydroxymethyl-12-crown-4 and anhydrous chloroform to prepare a mixed solution with a molar ratio of 1:4; add 0.4 mol of triethylamine and mix well; dropwise add 0.3 mol of 2-acryloyl chloride to carry out esterification reaction, and react at 20° C. for 4 hours; after the reaction, separate and purify the product by column chromatography, the column chromatography material is 100-200 mesh chromatography silica gel, the eluent is a mixture of petroleum ether and ethyl acetate in a volume ratio of 2:1, perform chromatography separation and purification, collect the purified product eluent and distill under reduced pressure to obtain 12-crown-4-2-fluoro-2-acrylic acid methyl ester.
[0087] Then, an acrylate crown polymer was prepared, and 0.1 mol of the prepared 12-crown-4-2-fluoro-2-methyl acrylate was weighed and mixed with anhydrous methanol to prepare a mixed solution with a molar ratio of 1:0.7; 0.001 mol of azobisisobutyronitrile was added in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution, and the reaction was carried out at 70°C for 6 hours; after the reaction was completed, the solid precipitate was distilled under reduced pressure to obtain a solid precipitate, which was repeatedly washed with the corresponding anhydrous methanol and freeze-dried to obtain poly-12-crown-4-2-fluoro-2-methyl acrylate. The number average molecular weight (Mn) of the obtained poly-12-crown-4-2-fluoro-2-methyl acrylate was 6700 after analysis by gel permeation chromatography (GPC).
[0088]
Example 5
[0089] First, prepare an ester crown ether monomer, weigh 0.2 mol of 2-hydroxymethyl-15-crown-5 and anhydrous ethanol to prepare a mixed solution with a molar ratio of 1:3; add 0.2 mol of triethylamine and mix well; add 0.3 mol of methacryloyl chloride dropwise for esterification reaction at 0°C for 4 hours; after the reaction, separate and purify the product by column chromatography, the column chromatography material is 100-200 mesh chromatography silica gel, the eluent is a mixture of petroleum ether and ethyl acetate in a volume ratio of 1:2, separate and purify by chromatography, collect the purified product eluent and distill under reduced pressure to obtain 15-crown-5-2-methyl methacrylate.
[0090] Then, an ester crown polymer was prepared, and 0.1 mol of the prepared 15-crown-5-2-methyl methacrylate was weighed and mixed with anhydrous N,N-dimethylformamide to prepare a mixed solution with a molar ratio of 1:0.5; 0.002 mol of diisopropylbenzene peroxide was added in a saturated nitrogen atmosphere with a water-oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution, and the reaction was carried out at 60°C for 10 hours; after the reaction was completed, the solid precipitate was distilled under reduced pressure to obtain a solid precipitate, which was repeatedly washed with the corresponding anhydrous N,N-dimethylformamide, and freeze-dried to obtain poly-15-crown-5-2-methyl methacrylate. The number average molecular weight (Mn) of the obtained poly-15-crown-5-2-methyl methacrylate was 6700 after analysis by gel permeation chromatography (GPC).
[0091] [Comparative Example]
[0092] Conventional unmodified aluminum-based adsorbents were prepared using a co-precipitation method.
[0093] First, 0.5 mol LiCl and 1.0 mol AlCl3 were weighed and placed in 100 ml water, and mixed and dissolved completely to obtain a lithium aluminum aqueous solution; then, 20 ml of a 6 mol / L NaOH solution was prepared and heated to 80°C; the lithium aluminum aqueous solution was then added dropwise to the high-speed stirred NaOH solution at a stirring speed of 350 rpm, and the temperature was maintained at 80°C for a full reaction of 1 hour, and a solid precipitate was obtained by vacuum distillation, which was then washed with distilled water for several times and freeze-dried to obtain [LiAl2(OH)6]X n- 1-n mH2O aluminum-based adsorbent.
[0094] [Simulation test of lithium extraction from salt lake]
[0095] Simulated salt lake brine: Na + 98.01g / L, Mg 2+ 17.1g / L, Li + 0.78g / L, Cl - 191.3g / L, Ca 2+ 0.12g / L, K + 16.7g / L, SO4 2- 21.9g / L, pH 7.24.
[0096] Test method:
[0097] The adsorbent materials were placed in a group of simulated salt lake brine (pre-adsorption solution) and stirred for adsorption at a temperature of 15°C, a stirring speed of 300 r / min, and an adsorption time of 2 h. After the adsorption was completed, vacuum filtration was performed to obtain the post-adsorption solution and the loaded adsorbent material.
[0098] Take the above-mentioned loaded adsorbent material, and desorb it with a hydrochloric acid solution with a concentration of 0.5 mol / L at a rotation speed of 300 r / min and a desorption time of 2 h. After the desorption is completed, vacuum filtration is performed to obtain a desorption solution and an unloaded adsorbent material.
[0099] The ICP-MS method was used to determine the element concentrations in the solution before adsorption, the solution after adsorption, and the desorption solution. The adsorption capacity of the adsorbent material for lithium ions was calculated according to the following formula:
[0100] Q t =(C0-C t )×V / m
[0101] Among them, Q t ——Adsorption capacity, C0——Lithium ion concentration of solution before adsorption, C t ——Lithium ion concentration of the solution after adsorption, V——volume of the solution, m——mass of the adsorption material.
[0102] The acrylate crown ether polymers obtained in Examples 1 to 5 and the conventional unmodified aluminum-based adsorbent prepared by the coprecipitation method in the comparative example were used to conduct a simulation test on lithium extraction from salt lakes. The test results are shown in Tables 1 and 2.
[0103] Table 1 Adsorption capacity of adsorbent materials for lithium ions, mg / g
[0104]
[0105] Table 2 Element concentrations in analytical solutions, g / L
[0106]
[0107] Test conclusion:
[0108] 1. The adsorption capacity of the enoate crown ether polymer of the present invention for lithium ions can reach 36.07 mg / g, which has obvious advantages over the existing lithium extraction adsorbents. The enoate crown ether polymer of the present invention is based on a crown ether segment polymer, which is directly polymerized from a crown ether derivative body. The crown ether functional group density is large, the adsorption sites are many, and the adsorption capacity for lithium ions is large. On the other hand, the main chain of the enoate crown ether polymer uses a rigid connecting group, which improves the rigidity of the main chain and further improves the ability of the enoate crown ether polymer to capture lithium ions.
[0109] 2. The acrylate crown ether polymer of the present invention preferably has an acrylate crown ether derivative monomer of acrylate-12-crown-4 monomer, whose crown ether ring cavity diameter is comparable to that of lithium ions, and has a strengthening effect of the ester group, has a specific adaptability to lithium ions, and improves its selective separation ability.
[0110] 3. The enoate crown ether polymer of the present invention is a crown ether derivative bulk polymer, and its mechanical and thermal properties are greatly improved, and it has good stability and strong adaptability to the environment.
[0111] In summary, the acrylate crown ether polymer of the present invention is applied to separate and enrich lithium ions in salt lake brine and has broad application prospects.
[0112] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. An acrylate crown ether polymer, characterized in that The acrylate crown ether polymer is composed of the following repeating structural units: acrylate crown ether, and has a number average molecular weight of 6700 to 15000. Wherein, m is the number of repetitions of ethoxy groups in the crown ether ring, n is the number of repetitions of the enoate crown ether, and R1 and R2 are linking groups on the enoate crown ether.
2. The acrylate crown ether polymer according to claim 1, characterized in that The repetition number m of the ethoxy group in the crown ether ring includes 1, 2 and 3, that is, the acrylate crown ether includes acrylate 12 crown 4, acrylate 15 crown 5 and acrylate 18 crown 6. Preferably, the repetition number m of the ethoxy group in the crown ether ring is 1, that is, the acrylate crown ether is acrylate 12 crown 4.
3. The acrylate crown ether polymer according to claim 2, characterized in that: The linking group R1 on the enoate crown ether includes CH3-, F, and H, and R2 includes CH3-, H, preferably R1=CH3- or F, or R2=CH3-.
4. A method for synthesizing the acrylate crown ether polymer as claimed in claims 1 to 3, comprising the following steps: A. preparing an acrylate crown ether monomer, comprising: (A1) weighing 2-hydroxymethyl-crown ether and an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:1 to 4; (A2) adding 1 to 2 times the amount of 2-hydroxymethyl-crown ether substance as esterification aid and mixing evenly; (A3) adding 1 to 1.5 times the amount of 2-hydroxymethyl-crown ether substance in an amount of acyl chloride derivative to carry out esterification reaction at 0°C to 20°C for 1 hour to 2 hours; (A4) After the reaction is completed, the product is separated and purified by column chromatography, the column chromatography material is selected from 100-300 mesh chromatography silica gel, the eluent is selected from a mixture of petroleum ether and ethyl acetate, the chromatography separation and purification is performed, and the eluent of the purified product is collected and distilled under reduced pressure to obtain an ester crown ether monomer, the chemical structure of which is: Wherein, m is the number of repetitions of ethoxy groups in the crown ether ring, and R1 and R2 are linking groups on the enoate crown ether. B Preparation of acrylate crown ether polymers (B1) weighing the acrylate crown ether monomer prepared in step A and mixing it with an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:0.5 to 1; (B2) adding 1% to 10% of a free radical polymerization initiator in a saturated nitrogen atmosphere with a water oxygen concentration of less than 50 ppm to initiate a free radical polymerization reaction of the mixed solution at 40° C. to 70° C. for 6 h to 24 h; (B3) After the reaction is completed, the solid precipitate is distilled under reduced pressure to obtain a solid precipitate, which is washed with the corresponding anhydrous organic solvent in step B1 for more than 3 times and dried to obtain the enoate crown ether polymer.
5. The synthesis method according to claim 4, characterized in that The anhydrous organic solvent includes methanol, ethanol, dichloromethane, chloroform, tetrahydrofuran, N,N-dimethylformamide or a mixture thereof.
6. The synthesis method according to claim 4, characterized in that The 2-hydroxymethyl-crown ethers in step A include 2-hydroxymethyl-12-crown-4, 2-hydroxymethyl-15-crown-5 and 2-hydroxymethyl-18-crown-6, and their general chemical structures are as follows: Here, m is the number of repetitions of the ethoxy group in the crown ether ring.
7. The synthesis method according to claim 4, characterized in that The esterification auxiliary agent in step A includes sodium carbonate, sodium hydroxide, ammonia water and triethylamine.
8. The synthesis method according to claim 4, characterized in that The acyl chloride derivatives described in step A include acryloyl chloride, crotonyl chloride, 2-fluoroacryloyl chloride and methacryloyl chloride, and their general chemical structures are as follows: Among them, R1 includes CH3-, F, and H, and R2 includes CH3- and H.
9. The synthesis method according to claim 4, characterized in that The mixed solution of petroleum ether and ethyl acetate in step A includes a mixed solution with a volume ratio of 1-2:1-2.
10. The synthesis method according to claim 4, characterized in that: The free radical polymerization initiator in step B includes potassium persulfate, azobisisobutyronitrile and diisopropylbenzene peroxide.
11. An application of an acrylate crown ether polymer, characterized in that: The enoate crown ether polymers according to claims 1 to 3, and the enoate crown ether polymers prepared by the synthesis methods according to claims 4 to 10, are used for separating and enriching lithium ions in salt lake brine.
Citation Information
Cited By
Sepiolite-based lithium ion imprinted polymer, preparation method and application in adsorption and separation of lithium ions in low-grade brine
CN122647654A