Preparation of silver chloride nanosphere catalyst and application of silver chloride nanosphere catalyst in production of CO by electrochemical reduction of CO2

By preparing silver chloride nanosphere catalyst, the problem of low CO selectivity of electroreduction of CO2 is solved, and efficient and stable CO2 reduction catalysis is achieved, which is suitable for industrial applications.

CN118957642APending Publication Date: 2024-11-15JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411252036.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, CO2 electroreduction produces CO2 with low selectivity, low current density and low utilization rate, which limits its application in the energy field.

Method used

A method of preparing a silver chloride nanosphere catalyst is adopted to form AgCl nanospheres by stirring polyvinylpyrrolidone, silver nitrate, potassium bicarbonate and potassium pyrophosphate in ultrapure water and sonicating it, and then forming AgCl nanospheres on carbon paper. After loading, negative potential electrolysis is applied to the KHCO3 solution to obtain an efficient CO2 reduction catalyst.

Benefits of technology

It has achieved high electrocatalytic efficiency and high stability. The Faraday efficiency of electrochemical CO2 reduction to produce CO has reached more than 90%. It has a simple process, green and environmentally friendly, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957642A_ABST
    Figure CN118957642A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalyst preparation, and particularly relates to preparation of a silver chloride nanosphere catalyst and application of the silver chloride nanosphere catalyst to production of CO through electrochemical reduction of CO2. Polyvinylpyrrolidone, silver nitrate, potassium bicarbonate and potassium pyrophosphate solids are sequentially put into an ultra-pure water solution, and a mixed solution A is obtained; uniformly stirring, adding a sodium chloride solution, uniformly stirring, performing centrifugal separation to obtain a solid, washing, and performing vacuum drying to obtain AgCl nanospheres; mixing AgCl nanospheres with the mixed solution B to obtain a mixed solution C; performing ultrasonic treatment on the mixed solution C at normal temperature, dropwise adding the mixed solution C subjected to ultrasonic treatment onto carbon paper, and drying under an infrared lamp to obtain carbon paper loaded with AgCl nanospheres; and placing the carbon paper loaded with the AgCl nanospheres in a KHCO3 solution as a cathode, and applying negative potential to obtain the working electrode material. The silver chloride nanosphere catalyst prepared by the method shows excellent electrochemical performance, and has relatively high electro-catalytic efficiency and good cycle stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, in particular to the preparation of a silver chloride nanosphere catalyst and its application in electrochemical reduction of CO2 to produce CO. Background Art

[0002] In order to control carbon dioxide emissions and solve the problems caused by excessive carbon dioxide emissions, a large number of researchers have focused on the energy field, capturing and collecting carbon dioxide through various methods and then converting carbon dioxide into high-value chemicals through catalysis (such as chemical, photochemical catalysis, thermal catalysis, electrochemical catalysis of carbon dioxide, etc.), among which carbon monoxide is widely used in chemical industry, metallurgy and other fields, and is the main component of synthesis gas and an important raw material for organic chemical products; in addition, because carbon monoxide has reducing properties, it is also used as a reducing agent for refining metals, but the current source of carbon monoxide is mainly the incomplete combustion of carbon-containing fuels. Therefore, the process of electrochemical reduction of CO2 to produce CO products plays a vital role in eliminating the current situation of production and life relying on fossil fuels and meeting the increasing energy supply.

[0003] So far, people have made great efforts in the electrochemical reduction of CO2 to CO, but the low product selectivity, low current density, and low utilization rate of CO2 in the reduction process have limited its application. Therefore, it is of great significance to develop highly active and highly selective catalysts for electrochemical CO2 to CO products.

[0004] Based on the above problems, we propose a preparation method of silver chloride nanosphere catalyst and its application in electrochemical reduction of CO2 to produce CO. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of the embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0006] In view of the problems existing in the prior art, the present invention is proposed.

[0007] Therefore, the purpose of the present invention is to provide a preparation of a silver chloride nanosphere catalyst and its application in the electrochemical reduction of CO2 to produce CO. The prepared silver chloride nanospheres are used for electrocatalytic CO2 reduction to produce CO and have high electrocatalytic efficiency and high stability.

[0008] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0009] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0010] The first object of the present invention is to provide a method for preparing a silver chloride nanosphere catalyst, comprising the following steps:

[0011] S1. Put polyvinyl pyrrolidone, silver nitrate and potassium bicarbonate solids in a mass ratio of 6:1:2 into an ultrapure aqueous solution in turn, stir until the solids are completely dissolved, then add potassium pyrophosphate, ultrasonicate and stir until the solids are completely dissolved, to obtain a mixed solution A;

[0012] S2, adding sodium chloride solution to the obtained mixed solution A, stirring, centrifuging to obtain a solid, washing the obtained solid with ultrapure water and anhydrous ethanol respectively, and then vacuum drying to obtain AgCl nanospheres;

[0013] S3, mixing the obtained AgCl nanospheres with mixed solution B in a mass ratio of 1:(50-150) to obtain a mixed solution C, wherein the obtained mixed solution B consists of ultrapure water, anhydrous ethanol and naphthol in a volume ratio of (3-6):(3-6):1, performing ultrasonic treatment on the mixed solution C at room temperature, dropping the ultrasonically treated mixed solution C onto carbon paper, and drying under an infrared lamp to obtain carbon paper loaded with AgCl nanospheres;

[0014] S4. The obtained carbon paper loaded with AgCl nanospheres is placed as a cathode in a KHCO3 solution, CO2 gas is introduced, and a negative potential is applied for electrolysis for 20 minutes to obtain a cathode electrode material.

[0015] The method for preparing the silver chloride nanosphere catalyst according to patent claim 1 is characterized in that the potassium pyrophosphate in step S1 is 3-6 g.

[0016] Preferably, the sodium chloride solution in step S2 is 1-3 ml of 0.5 M sodium chloride solution.

[0017] Preferably, the stirring time of step S2 is 1-3h.

[0018] Preferably, in step S1 and step S3, the ultrasonic treatment time is 10-20 min.

[0019] Preferably, the vacuum drying temperature in step S2 is 30-60°C.

[0020] Preferably, in step S4, the negative potential applied is -0.6 to -0.9 V vs. RHE.

[0021] The second object of the present invention is to provide a silver chloride nanosphere catalyst prepared by the above preparation method.

[0022] The third object of the present invention is to provide an application of a silver chloride nanosphere catalyst in the electroreduction of CO2 to produce CO, specifically, comprising the following steps: using AgCl nanosphere electrode material as a working electrode, using Ag / AgCl and Pt mesh as a reference electrode and a counter electrode respectively, and using a KHCO3 solution as an electrolyte; then, electrolyzing and reducing CO2 at an electrolysis voltage of -0.7 to -1.1 V vs. RHE to obtain CO.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) The preparation method provided by the present invention has a simple process, mild reaction, and the entire process is green and environmentally friendly, which provides support for industrial production.

[0025] (2) The silver chloride nanospheres prepared by the present invention exhibit excellent electrochemical performance, high electrocatalytic efficiency, good cycle stability and excellent Faradaic efficiency (FE). BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the present invention will be described in detail below in combination with the accompanying drawings and detailed embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0027] Figure 1 The X-ray diffraction spectra of Example 1 (AgCl nanospheres), Comparative Example 1 (AgBr nanospheres), and Comparative Example 2 (Ag nanospheres);

[0028] Figure 2 The figures are scanning electron microscope images of the AgCl nanospheres (a) prepared in Example 1, the AgBr nanospheres (c) prepared in Comparative Example 1, and the Ag nanospheres (e) prepared in Comparative Example 2, and the particle size distributions of the AgCl nanospheres (b) prepared in Example 1, the AgBr nanospheres (d) prepared in Comparative Example 1, and the Ag nanospheres (f) prepared in Comparative Example 2;

[0029] Figure 3 The X-ray photoelectron spectra of the AgCl nanospheres (a) prepared in Example 1 and the AgBr nanospheres (b) prepared in Comparative Example 1 are shown;

[0030] Figure 4 The X-ray diffraction spectra of Cl-Ag, Br-Ag and Ag obtained after electro-reduction of Example 1 (AgCl nanospheres), Comparative Example 1 (AgBr nanospheres) and Comparative Example 2 (Ag nanospheres);

[0031] Figure 5 , Figure 6 It is the X-ray photoelectron spectra of Cl-Ag, Br-Ag and Ag obtained after electro-reduction of Example 1 (AgCl nanospheres), Comparative Example 1 (AgBr nanospheres) and Comparative Example 2 (Ag nanospheres);

[0032] Figure 7 is a transmission electron microscope image of the AgCl nanospheres prepared in Example 1 after electroreduction;

[0033] Figure 8 The voltammograms of Application Example 1 (AgCl nanospheres), Comparative Application Example 1 (AgBr nanospheres) and Comparative Application Example 2 (Ag nanospheres) in inert gas Ar and in 0.5M KHCO3 saturated with CO2;

[0034] Fig. 9 It is a Faraday efficiency diagram of electrochemical CO2 reduction to CO production at different potentials for Application Example 1 (AgCl nanospheres), Comparative Application Example 1 (AgBr nanospheres) and Comparative Application Example 2 (Ag nanospheres);

[0035] Fig.10 This is a graph showing the long-term electrolysis performance of the AgCl nanospheres prepared in Application Example 1 under a given current. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0037] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0038] Secondly, the present invention is described in detail with reference to schematic diagrams. When describing the embodiments of the present invention in detail, for the sake of convenience, the cross-sectional diagrams showing the device structure will not be partially enlarged according to the general scale, and the schematic diagrams are only examples, which should not limit the scope of protection of the present invention. In addition, in actual production, the three-dimensional dimensions of length, width and depth should be included.

[0039] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.

[0040] The present invention provides the following technical solutions: preparation of a silver chloride nanosphere catalyst and application in electrochemical reduction of CO2 to produce CO, wherein the prepared silver chloride nanosphere is applied to electrocatalytic reduction of CO2 to produce CO, and has high electrocatalytic efficiency and high stability;

[0041] Example 1

[0042] S1. Weigh 600 mg of polyvinyl pyrrolidone, 100 mg of silver nitrate, and 200 mg of potassium bicarbonate solid, put them into 40 ml of ultrapure aqueous solution in sequence, stir until the solid is completely dissolved, add 4.5 g of potassium pyrophosphate, and stir for 20 minutes with ultrasound until the solid is completely dissolved to obtain a mixed solution A;

[0043] S2, adding 1 ml of sodium chloride solution to the obtained mixed solution A, stirring for 1 hour, and centrifuging to obtain a solid, and washing the obtained solid with ultrapure water and anhydrous ethanol respectively, and vacuum drying at 60° C. to obtain AgCl nanospheres;

[0044] S3, take 5 mg of AgCl nanospheres and mix them with 250 μL ultrapure water and 250 μL ethanol, and add 50 μL naphthalene, and perform ultrasonic treatment for 20 min at room temperature, add the mixed solution C after ultrasonic treatment for 20 min dropwise on carbon paper, and dry under infrared lamp to obtain carbon paper loaded with AgCl nanospheres;

[0045] S4. The obtained carbon paper loaded with AgCl nanospheres was placed as a cathode in a KHCO3 solution, CO2 gas was introduced to exhaust the air inside the solution and allow CO2 to fully dissolve, and a negative potential (-1.4 V vs. RHE) was applied for electrolysis for 20 minutes to obtain the cathode electrode material Cl-Ag.

[0046] Example 2

[0047] S1. Weigh 600 mg of polyvinyl pyrrolidone, 100 mg of silver nitrate, and 200 mg of potassium bicarbonate solid, put them into 40 ml of ultrapure aqueous solution in sequence, stir until the solid is completely dissolved, add 3 g of potassium pyrophosphate, and stir and sonicate for 10 min until the solid is completely dissolved to obtain a mixed solution A;

[0048] S2, adding 2 ml of sodium chloride solution to the obtained mixed solution A, stirring for 2 h, and centrifuging to obtain a solid, washing the obtained solid with ultrapure water and anhydrous ethanol respectively, and vacuum drying at 40° C. to obtain AgCl nanospheres;

[0049] S3, take 5 mg of AgCl nanospheres, mix them with 250 μL ultrapure water and 250 μL ethanol, add 50 μL naphthalene, and perform ultrasonic treatment for 10 min at room temperature, add the mixed solution C after ultrasonic treatment for 10 min dropwise on carbon paper, and dry it under infrared lamp to obtain carbon paper loaded with AgCl nanospheres;

[0050] S4. The obtained carbon paper loaded with AgCl nanospheres was placed as a cathode in a KHCO3 solution, CO2 gas was introduced to exhaust the air inside the solution and allow CO2 to fully dissolve, and a negative potential (-1.2 V vs. RHE) was applied for electrolysis for 20 minutes to obtain the cathode electrode material Cl-Ag.

[0051] Example 3

[0052] S1. Weigh 600 mg of polyvinyl pyrrolidone, 100 mg of silver nitrate, and 200 mg of potassium bicarbonate solid, put them into 40 ml of ultrapure aqueous solution in sequence, stir until the solid is completely dissolved, add 6 g of potassium pyrophosphate, and stir and sonicate for 10 min until the solid is completely dissolved to obtain a mixed solution A;

[0053] S2, adding 3 ml of sodium chloride solution to the obtained mixed solution A, stirring for 3 hours, and centrifuging to obtain a solid, and washing the obtained solid with ultrapure water and anhydrous ethanol respectively, and vacuum drying at 40° C. to obtain AgCl nanospheres;

[0054] S3, take 5 mg of AgCl nanospheres, mix them with 250 μL ultrapure water and 250 μL ethanol, add 50 μL naphthalene, and perform ultrasonic treatment for 10 min at room temperature, add the mixed solution C after ultrasonic treatment for 10 min dropwise on carbon paper, and dry it under infrared lamp to obtain carbon paper loaded with AgCl nanospheres;

[0055] S4. The obtained carbon paper loaded with AgCl nanospheres was placed as a cathode in a KHCO3 solution, CO2 gas was introduced to exhaust the air inside the solution and allow CO2 to fully dissolve, and a negative potential (-1.5 V vs. RHE) was applied for electrolysis for 20 minutes to obtain the cathode electrode material Cl-Ag.

[0056] Comparative Example 1

[0057] S1. Weigh 600 mg of polyvinyl pyrrolidone, 100 mg of silver nitrate, and 200 mg of potassium bicarbonate solid, put them into 40 ml of ultrapure aqueous solution in sequence, stir until the solid is completely dissolved, add 4.5 g of potassium pyrophosphate, and stir for 20 minutes with ultrasound until the solid is completely dissolved to obtain a mixed solution A;

[0058] S2, adding 1 ml of sodium bromide solution to the obtained mixed solution A, stirring for 1 hour, and centrifuging to obtain a solid, washing the obtained solid with ultrapure water and anhydrous ethanol respectively, and vacuum drying at 60° C. to obtain AgBr nanospheres;

[0059] S3, take 5 mg of AgBr nanospheres, mix them with 250 μL ultrapure water and 250 μL ethanol, add 50 μL naphthalene, and perform ultrasonic treatment for 20 min at room temperature, drop the mixed solution C after ultrasonic treatment for 20 min on carbon paper, and dry it under infrared lamp to obtain carbon paper loaded with AgBr nanospheres;

[0060] S4. The obtained carbon paper loaded with AgBr nanospheres was placed as a cathode in a KHCO3 solution, CO2 gas was introduced to exhaust the air inside the solution and allow CO2 to fully dissolve, and a negative potential (-1.4 V vs. RHE) was applied for electrolysis for 20 minutes to obtain a cathode electrode material Br-Ag.

[0061] Comparative Example 2

[0062] S1. Weigh 600 mg of polyvinyl pyrrolidone and 100 mg of silver nitrate, put them into 40 ml of ultrapure water solution in sequence, stir until the solid is completely dissolved, add 1 g of ascorbic acid, ultrasonically stir and treat for 20 min until the solid is completely dissolved to obtain a mixed solution A, stir for 1 h, and centrifuge to obtain a solid. The obtained solid is washed with ultrapure water and anhydrous ethanol respectively, and then vacuum dried at 60° C. to obtain Ag nanospheres;

[0063] S2, take 5 mg of Ag nanospheres, mix them with 250 μL ultrapure water and 250 μL ethanol, add 50 μL naphthalene, and perform ultrasonic treatment for 20 min at room temperature, add the mixed solution C after ultrasonic treatment for 20 min dropwise on carbon paper, and dry it under infrared lamp to obtain carbon paper loaded with Ag nanospheres;

[0064] S3. The obtained carbon paper loaded with Ag nanospheres was placed as a cathode in a KHCO3 solution, CO2 gas was introduced to exhaust the air inside the solution and allow CO2 to fully dissolve, and a negative potential (-1.4 V vs. RHE) was applied for electrolysis for 20 minutes to obtain the cathode electrode material Ag.

[0065] The catalysts prepared by the methods of Example 1, Comparative Example 1 and Comparative Example 2 were used as samples, and X-ray diffraction (XRD), scanning electron microscopy (SEM) and particle size distribution were tested. The results are shown in the attached Figure 1 , as shown in 2.

[0066] refer to Figure 1 , X-ray diffraction analysis (XRD) results show that the diffraction peak positions of each prepared catalyst correspond to the standard PDF card peaks, confirming the successful synthesis of AgCl, AgBr and Ag;

[0067] refer to Figure 2The results of scanning electron microscopy (SEM) show that the particle size of the catalyst in Example 1 is relatively small and evenly distributed, mainly ranging from 57 to 84 nm, which is more evenly distributed than the particle size of the catalyst in Comparative Example 1 and smaller than the particle size of the catalyst in Comparative Example 2;

[0068] refer to Figure 3 X-ray photoelectron spectroscopy (XPS) analysis shows that silver is Ag in Example 1 and Comparative Example 1. + ;

[0069] refer to Figure 4 , X-ray diffraction analysis (XRD) results of the Cl-Ag, Br-Ag and Ag electrodes prepared after electro-reduction showed that the catalysts of Example 1, Comparative Example 1 and Comparative Example 2 existed as Ag;

[0070] refer to Figure 5 , 6, X-ray photoelectron spectroscopy (XPS) analysis of the Cl-Ag, Br-Ag and Ag electrodes obtained after electroreduction showed that the silver in the catalysts of Example 1, Comparative Example 1 and Comparative Example 2 was Ag. 0 , while the presence of Cl in Cl-Ag and Br in Br-Ag species proves the residual Cl and Br after electroreduction.

[0071] refer to Figure 7 ,The transmission electron microscopy (TEM) results show that the catalyst of Example 1 can maintain the structure of nanospheres after electrochemical reduction.

[0072] Application Example 1

[0073] In the H-type electrolytic cell, the Cl-Ag obtained after the electrochemical reduction in Example 1 was used as the working electrode, Ag / AgCl and Pt mesh were used as the reference electrode and the counter electrode, respectively, and a 0.5M KHCO3 solution was used as the electrolyte. The cathode cell and the anode cell of the H-type electrolytic cell were separated by a proton exchange membrane, and electrochemical CO2 reduction to generate CO was carried out in the working electrode range of -0.7 to -1.1 V vs. RHE. Figure 8 The current density of the AgCl nanospheres prepared in Example 1 is given. Fig. 9 The Faraday efficiency of the electrochemical carbon dioxide reduction to carbon monoxide of the AgCl nanospheres prepared in Example 1 at different potentials is given by Fig. 9 It can be seen that the AgCl nanospheres prepared in Example 1 have good product selectivity in the electrochemical CO2 reduction reaction to generate CO, and their FE is greater than 90% in a wide potential range (-0.7 to -1.1 V vs. RHE). In a flow-type electrolytic cell, the Cl-Ag obtained after electrochemical reduction in Example 1 was used as a working electrode, Ag / AgCl and Pt mesh were used as reference electrodes and counter electrodes, respectively, and 1M KOH solution was used as an electrolyte. Fig.10 The AgCl nanospheres prepared in Example 1 in a flow-type electrolytic cell at 200 mA / cm 2 The electrolysis was carried out for 20 h at the current density without obvious performance degradation.

[0074] Application Comparative Example 1

[0075] In the H-type electrolytic cell, the Br-Ag obtained after electrochemical reduction in Comparative Example 1 was used as a working electrode, Ag / AgCl and Pt mesh were used as a reference electrode and a counter electrode, respectively, a 0.5 M KHCO3 solution was used as an electrolyte, and a proton exchange membrane was used to separate the cathode cell and the anode cell of the H-type electrolytic cell. Electrochemical CO2 reduction to generate CO was carried out in the working electrode range of -0.7 to -1.1 V vs. RHE.

[0076] Application Comparative Example 2

[0077] In the H-type electrolytic cell, the Ag obtained after the electrochemical reduction of Comparative Example 2 was used as the working electrode, Ag / AgCl and Pt mesh were used as the reference electrode and the counter electrode, respectively, and a 0.5M KHCO3 solution was used as the electrolyte. The cathode pool and the anode pool of the H-type electrolytic cell were separated by a proton exchange membrane, and electrochemical CO2 reduction to generate CO was carried out in the working electrode range of -0.7 to -1.1 V vs. RHE.

[0078] Figure 8 The voltammograms of the catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2 in inert gas Ar and in 0.5M KHCO3 saturated with CO2 are shown in FIG. Figure 8 It can be seen that the catalyst prepared in Example 1 has the best current density; Fig. 9 is the Faraday efficiency of electrochemical carbon dioxide reduction to carbon monoxide at different potentials for the catalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2, and is Fig. 9 It can be seen that the catalyst prepared in Example 1 has the best CO Faraday efficiency.

[0079] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for preparing a silver chloride nanosphere catalyst, characterized in that: The following steps are involved: S1. Put polyvinyl pyrrolidone, silver nitrate and potassium bicarbonate solids in a mass ratio of 6:1:2 into an ultrapure aqueous solution in turn, stir until the solids are completely dissolved, then add potassium pyrophosphate, ultrasonicate and stir until the solids are completely dissolved, to obtain a mixed solution A; S2, adding sodium chloride solution to the obtained mixed solution A, stirring, centrifuging to obtain a solid, washing the obtained solid with ultrapure water and anhydrous ethanol respectively, and then vacuum drying to obtain AgCl nanospheres; S3, mixing the obtained AgCl nanospheres with mixed solution B in a mass ratio of 1:(50-150) to obtain a mixed solution C, wherein the obtained mixed solution B consists of ultrapure water, anhydrous ethanol and naphthol in a volume ratio of (3-6):(3-6):1, performing ultrasonic treatment on the mixed solution C at room temperature, dropping the ultrasonically treated mixed solution C onto carbon paper, and drying under an infrared lamp to obtain carbon paper loaded with AgCl nanospheres; S4. The obtained carbon paper loaded with AgCl nanospheres is placed as a cathode in a KHCO3 solution, CO2 gas is introduced, and a negative potential is applied for electrolysis for 20 minutes to obtain a cathode electrode material.

2. The method for preparing the silver chloride nanosphere catalyst according to claim 1, characterized in that: The potassium pyrophosphate in step S1 is 3-6 g.

3. The method for preparing the silver chloride nanosphere catalyst according to claim 1, characterized in that: The sodium chloride solution in step S2 is 1-3 ml of 0.5 M sodium chloride solution.

4. The method for preparing the silver chloride nanosphere catalyst according to claim 1, characterized in that: The stirring time of step S2 is 1-3h.

5. The method for preparing the silver chloride nanosphere catalyst according to claim 1, characterized in that: In step S1 and step S3, the ultrasonic treatment time is 10-20 min.

6. The method for preparing the silver chloride nanosphere catalyst according to claim 1, characterized in that: The vacuum drying temperature in step S2 is 30-60°C.

7. The method for preparing the silver chloride nanosphere catalyst according to claim 1, characterized in that: In the step S4, the negative potential applied is -0.6 to -0.9 V vs. RHE.

8. A silver chloride nanosphere catalyst prepared by the preparation method as described in any one of claims 1 to 6.

9. Use of the silver chloride nanosphere catalyst as claimed in claim 7 in the electroreduction of CO2 to produce CO.

10. The use of the silver chloride nanosphere catalyst in electroreduction of CO2 to produce CO according to claim 8, characterized in that: The following steps are involved: AgCl nanosphere electrode material is used as the working electrode, Ag / AgCl and Pt mesh are used as the reference electrode and counter electrode respectively, and KHCO3 solution is used as the electrolyte; then, CO2 is electrolytically reduced at an electrolysis voltage of -0.7 to -1.1 V vs. RHE to obtain CO.