Porous metal catalyst and preparation method thereof
By forming an alloy layer on a micron porous substrate and vacuum heat treatment, the problems of poor mechanical performance and insufficient catalytic efficiency of micro-nano porous metal catalytic electrodes in the electrolytic hydrogen production process are solved, and high-efficiency, low-cost and environmentally friendly porous are achieved Metal catalyst preparation improves catalytic activity and mechanical strength.
Patent Information
- Application Number
- CN202411021336.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the electrolytic hydrogen production process, micro-nano porous metal catalytic electrodes have problems such as poor mechanical properties, insufficient catalytic efficiency, complex preparation process, high cost, and environmental pollution.
Annealing and vacuum heat treatment are used to form porous metal catalysts by using a mixture of micron porous substrates and a second metal and filler. The catalytic activity and mechanical strength are improved through alloy layering and vacuum heat treatment, avoid subsequent processing and forming processes, reduce the use of chemical reagents and Environmental impact.
The catalytic activity and mechanical strength of porous metal catalysts are improved, the preparation time of alloy layer is shortened, the production cost is reduced, environmentally friendly large-scale production is achieved, the thickness of the alloy layer and the ligament size are controlled, and the specific surface area is improved.
Smart Images

Figure CN118957644A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrode materials, and in particular to a porous metal catalyst and a method for preparing the porous metal catalyst. Background Art
[0002] Compared with traditional micro-nano particles and bulk materials, micro-nano porous metals have many excellent physical and chemical properties, the root of which mainly comes from the unique structural characteristics of micro-nano porous metals, such as high porosity, large specific surface area, high electrical conductivity, adjustable composition-structure-size, etc. Therefore, the development of new micro-nano porous metals has always received widespread attention.
[0003] As a clean and efficient secondary energy source, hydrogen energy has the characteristics of high energy density (140MJ / kg), multiple preparation methods, storage, transportation, and wide application range. In addition, as an energy interconnection medium, hydrogen energy can also be produced through renewable energy, then stored on a large scale and used for peak load regulation, and finally realized through water circulation to achieve a closed loop of clean and pollution-free whole process and efficient energy storage / release, providing a feasible path for deep decarbonization in transportation, industry, construction and other fields.
[0004] Among the many hydrogen production processes, the use of renewable energy to produce hydrogen by electrolysis of water is recognized as the best way. As one of the most core components in the process of hydrogen production by electrolysis of water, the catalytic electrode is mostly in the form of metal mesh, metal foam and metal felt. The current mainstream catalytic electrode preparation processes are spraying and electroplating, but both generally have problems such as high overpotential of hydrogen evolution reaction or poor durability. The main reasons are the small number of catalytic active sites and the easy detachment of coating / electroplating layer. In recent years, when micro-nano porous metals prepared by the dealloying layer method act as catalytic electrodes or substrate materials in the water electrolysis process, they have shown excellent service performance due to their large specific surface area and self-supporting characteristics.
[0005] However, micro-nano porous metal catalytic electrodes still face many challenges in practical water electrolysis applications. For example, the method for preparing porous metal precursors is usually smelting-spinning or smelting-pressure processing. The precursor obtained by this method and the micro-nano porous metal obtained by the subsequent dealloying layer are generally difficult to meet the requirements of the morphology of the catalytic electrode in the electrolyzer (net-like, foam-like or felt-like). In addition, since the micro-nano porous metal is composed of a porous structure of micro-nano scale and has no solid matrix support, this will lead to poor overall mechanical properties of the porous metal, making it easy to collapse or decompose the overall structure in the hydrolysis process. Moreover, the vast majority of the dealloying layer processes for preparing micro-nano porous metal catalytic electrodes have many problems such as difficulty in expansion, long time consumption, high cost, the need for highly corrosive liquids during the production process, and easy environmental pollution.
[0006] In order to solve the above problems, the inventors of the present application proposed a porous metal catalyst and a method for preparing the porous metal catalyst. Summary of the invention
[0007] The present invention provides a porous metal catalyst and a method for preparing the porous metal catalyst, so as to solve the problems of poor mechanical properties and insufficient catalytic efficiency of a catalytic electrode with a porous structure.
[0008] According to a first aspect of the present invention, there is provided a method for preparing a porous metal catalyst, comprising:
[0009] providing a microporous substrate, a second metal, and a filler;
[0010] mixing the second metal and a filler to form a mixture;
[0011] Putting the micron porous substrate into an alloying device, wherein the micron porous substrate has a shape of a mesh, a foam or a felt;
[0012] Covering the mixture on the surface of the microporous substrate;
[0013] After covering the surface of the microporous substrate with the mixture, annealing the microporous substrate and the second metal to form an alloy layer on the surface of the microporous substrate;
[0014] The micron porous substrate with the alloy layer formed on the surface is placed in a vacuum heat treatment device for vacuum heat treatment to form a porous metal catalyst.
[0015] Optionally, during annealing treatment, the alloy layering temperature is 300°C to 500°C, and the holding time is 0.5h to 5h.
[0016] Optionally, the alloy layer has a thickness of 10 μm to 100 μm.
[0017] Optionally, the conditions for the vacuum heat treatment are: air pressure lower than 50 Pa, temperature range of 450° C. to 850° C., and insulation time of 0.5 h to 3.5 h.
[0018] Optionally, the size range of the ligaments in the porous metal catalyst is 100 nm to 2.5 μm.
[0019] Optionally, the filler includes: alumina or quartz sand.
[0020] Optionally, the second metal and the filler are in powder form.
[0021] Optionally, when the micron porous substrate is in a mesh or foam form, the mesh number of the micron porous substrate is 10 to 110 meshes; when the micron porous substrate is in a felt form, the wire diameter of the micron porous substrate is in a range of 3 μm to 100 μm.
[0022] Optionally, the particle size of the second metal is 120-325 mesh, and the particle size of the filler is 40-325 mesh.
[0023] Optionally, the mass ratio of the second metal to the filler is: the mixing ratio of the second metal to the filler is 1:1 to 1:3.
[0024] Optionally, the alloy layering equipment includes: a box furnace or a tube furnace.
[0025] Optionally, during the annealing treatment, a protective gas is introduced into the alloy layering equipment for 15 to 30 minutes before starting the heating, wherein the protective gas is argon or nitrogen.
[0026] Optionally, the micron porous substrate comprises a first characteristic metal, and after the alloy layer is formed on the surface of the micron porous substrate, the method further comprises:
[0027] The micron porous substrate with an alloy layer formed on the surface is placed in an acid solution for corrosion to obtain a metal catalyst with three-level porous characteristics.
[0028] Optionally, the first characteristic metal includes two or more micron porous base elements, and at least one element among the two or more micron porous base elements is Mn or Al.
[0029] Optionally, the acidic solution is ammonium sulfate.
[0030] Optionally, the concentration of ammonium sulfate is greater than or equal to 0.5M.
[0031] Optionally, the alloy layer includes a first metal element and a second metal element, the first metal element includes at least one of Ni, Fe, Cu, Co, Mn, Ti, Cr, Mo, W, Ta, Au, Ag, Nb, Zr, and V; the second metal element includes any one of Zn, Mg, Bi, and Cd.
[0032] According to a second aspect of the present invention, there is provided a method for preparing an electrode catalyst assembly, comprising the method for preparing the porous metal catalyst as described in any one of the first aspect of the present invention.
[0033] According to a third aspect of the present invention, there is provided a porous metal catalyst, comprising:
[0034] The micron porous substrate has an alloy layer formed by the first metal element and the second metal on its surface, the alloy layer also includes a filler, and the alloy layer has micro-nano pores.
[0035] Optionally, in the alloy layer, the molar percentage of the first metal element is 20%-50%; the molar percentage of the second metal element is 50%-80%.
[0036] Optionally, the alloy layer also includes nanoscale pores.
[0037] Optionally, the specific surface area of the porous metal catalyst is 75 to 95 m 2 / g.
[0038] Optionally, the hole size of the micron-scale porous substrate is 5 μm to 500 μm, the ligament size of the micro-nano porous substrate is 0.1 μm to 10 μm, and the ligament size of the nano-scale porous substrate is 10 nm to 99 nm.
[0039] According to a fourth aspect of the present invention, there is provided a catalytic electrode assembly comprising the porous metal catalyst according to the third aspect of the present invention.
[0040] According to a fifth aspect of the present invention, there is provided a use of the catalytic electrode assembly as described in the fourth aspect of the present invention in producing hydrogen by hydrolysis.
[0041] Optionally, the catalytic electrode assembly exhibits catalytic activity for oxygen evolution reaction.
[0042] Optionally, the catalytic electrode assembly exhibits catalytic activity for hydrogen evolution reaction.
[0043] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0044] The present invention provides a method for preparing a porous metal catalyst, which comprises covering the surface of the micron porous substrate with a second metal and a filler after being mixed evenly, and annealing the micron porous substrate and the second metal in an alloy layering device to form an alloy layer on the surface of the micron porous substrate, and placing the micron porous substrate with the alloy layer formed on the surface into a vacuum heat treatment device for vacuum heat treatment. Thus, the porous metal catalytic electrode prepared by the method only produces a porous structure in the alloy layer on the surface, so that while improving the activity of the porous metal catalyst, the micron porous substrate also ensures the mechanical strength of the formed porous metal catalyst. The technical solution provided by the present invention does not require subsequent processing and forming processes. Compared with gas phase alloy layering, the time required to prepare an alloy layer of the same thickness using the technical solution provided by the present invention is shorter and more efficient. In addition, the preparation method of the present invention does not require the use of various chemical reagents such as acids, alkalis and salts, and the sublimated metal vapor during the vacuum heat treatment process can be recovered by a condensing device and reused after treatment. Therefore, the experimental scheme provided by the present invention has less impact on the environment, lower production costs, and is easier to carry out large-scale production. Among them, the technical solution provided by the present invention can also realize the control of the thickness of the alloy layer and the size of the ligament. Specifically, by changing the time and temperature of the surface alloying layer, the thickness of the alloy layer can be controlled, and by controlling the temperature, duration and vacuum degree of the vacuum heat treatment, the size of the ligament of the porous structure can be controlled.
[0045] Furthermore, after the alloy layer is formed on the surface of the micron-scale porous substrate, the present invention places the micron-scale porous substrate containing the first characteristic metal into an acidic solution for corrosion, thereby forming nano-scale pores on the surface of the micro-nano-scale porous alloy layer, and forming a three-level porous catalyst structure on the micron-scale porous substrate, thereby greatly increasing the specific surface area of the porous metal catalyst, improving the catalytic activity, and ensuring the mechanical strength of the porous metal catalyst.
[0046] The present invention also provides a porous metal catalyst, which forms a micro-nano porous alloy layer on the surface of a micron porous substrate, thereby improving the activity of the porous metal catalyst, and the micron porous substrate ensures the mechanical strength of the porous metal catalyst. Therefore, the technical solution provided by the present invention improves the catalytic activity of the porous metal catalyst while also ensuring the mechanical strength of the porous metal catalyst structure.
[0047] Furthermore, the porous metal catalyst provided by the present invention also includes nanoscale pores, which form a three-level porous catalyst structure with the microscale pores in the micrometer porous substrate and the micro-nanoscale pores in the alloy layer, thereby increasing the specific surface area of the porous metal catalyst and greatly improving the catalytic activity of the porous metal catalyst. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0049] Figure 1 is a schematic flow chart of a method for preparing a porous metal catalyst provided in one embodiment of the present invention;
[0050] Figure 2 It is a cross-sectional scanning electron microscope image and an EDS element surface distribution image of a single wire after the surface alloy layering of the Ni mesh and the Zn powder in Example 1 of the present invention;
[0051] Figure 3 is a scanning electron microscope image of the micro-nano porous metal Ni mesh obtained after vacuum heat treatment in Example 1 of the present invention (the inset is a local enlarged image);
[0052] Figure 4 is the XRD diffraction pattern of the micro-nano porous metal Ni mesh obtained after vacuum heat treatment in Example 1 of the present invention;
[0053] Figure 5 It is a linear scanning diagram of the hydrogen evolution reaction on the surface of the micro-nano porous metal Ni mesh in Example 1 of the present invention;
[0054] Figure 6 It is a linear scanning diagram of the oxygen evolution reaction on the surface of the micro-nano porous metal Ni mesh in Example 1 of the present invention;
[0055] Figure 7 This is a scanning electron microscope image of the micro-nano porous metal Ni felt obtained after vacuum heat treatment in Example 2 of the present invention (the inset is a local magnified image);
[0056] Figure 8 This is a scanning electron microscope image of the micro-nano porous Ni-Cu alloy layer network obtained after vacuum heat treatment in Example 3 of the present invention (the inset is a local magnified image);
[0057] Fig. 9 is the XRD diffraction pattern of the micro-nano porous Ni-Cu alloy layer network obtained after vacuum heat treatment in Example 3 of the present invention;
[0058] Fig.10 This is a scanning electron microscope image of the micro-nano porous Ni-Mo-Cr-Fe alloy layer network obtained after vacuum heat treatment in Example 4 of the present invention (the inset is a local magnified image);
[0059] Fig.11is the XRD diffraction pattern of the micro-nano porous Ni-Mo-Cr-Fe alloy layer network obtained after vacuum heat treatment in Example 4 of the present invention;
[0060] Fig.12 This is a scanning electron microscope image of the micro-nano porous Ni-Fe-Cr alloy layer network obtained after vacuum heat treatment in Example 5 of the present invention (the inset is a local magnified image);
[0061] Fig.13 This is a transmission electron lattice contrast image of the metal catalyst having three-level porous features obtained after vacuum heat treatment and free corrosion in Example 6 of the present invention;
[0062] Fig.14 This is a scanning electron microscope image of a nickel mesh with Raney nickel sprayed on the surface in Comparative Example 1 of the present invention (the inset is a partial enlarged image);
[0063] Fig.15 This is a linear scanning diagram of the hydrogen evolution reaction on the surface of the nickel mesh sprayed with Raney nickel in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0064] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0065] The terms "first", "second", "third", "fourth", etc. (if any) in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0066] The technical solution of the present invention is described in detail with specific embodiments below. The following specific embodiments can be combined with each other, and the same or similar concepts or processes may not be described in detail in some embodiments.
[0067] Figure 1 A schematic flow chart of a method for preparing a porous metal catalyst provided by the present invention.
[0068] Please refer to Figure 1 According to one embodiment of the present invention, a method for preparing a porous metal catalyst is provided, comprising:
[0069] S11: providing a micron porous substrate, a second metal and a filler;
[0070] S12: mixing the second metal and the filler to form a mixture;
[0071] S13: placing the micron porous substrate into an alloying device, wherein the micron porous substrate has a mesh shape, a foam shape, or a felt shape;
[0072] S14: covering the mixture on the surface of the microporous substrate;
[0073] S15: after covering the surface of the microporous substrate with the mixture, annealing the microporous substrate and the second metal to form an alloy layer on the surface of the microporous substrate;
[0074] S16: placing the micron porous substrate having the alloy layer formed on the surface into a vacuum heat treatment device for vacuum heat treatment to form a porous metal catalyst.
[0075] The present invention provides a method for preparing a porous metal catalyst, which comprises covering the surface of the micron porous substrate with a second metal and a filler after being mixed evenly, and annealing the micron porous substrate and the second metal in an alloy layering device to form an alloy layer on the surface of the micron porous substrate, and placing the micron porous substrate with the alloy layer formed on the surface into a vacuum heat treatment device for vacuum heat treatment, so that the porous metal catalytic electrode prepared by this method only has a porous structure in the alloy layer on the surface, so that the micron porous substrate can ensure the mechanical strength of the formed porous metal catalyst while improving the activity of the porous metal catalyst. The technical solution provided by the present invention does not require subsequent processing and molding processes. Compared with gas phase alloy layering, the time required to prepare an alloy layer of the same thickness is shorter and more efficient.
[0076] The micron porous substrate is placed in an alloy layering device, and the second metal and filler mixed evenly are covered on the surface of the micron porous substrate. The micron porous substrate is in the shape of a mesh, foam or felt, and serves as a base metal.
[0077] The microporous substrate can be a mixed metal or a single metal.
[0078] In one embodiment, the micron porous substrate includes at least one of Ni, Fe, Cu, Co, Mn, Ti, Cr, Mo, W, Ta, Au, Ag, Nb, Zr, and V; and the second metal includes any one of Zn, Mg, Bi, and Cd.
[0079] The micron porous substrate is used to provide mechanical support for the porous metal catalyst, so that the porous metal catalyst finally prepared has high mechanical strength. Moreover, the porous metal catalyst formed by the micron porous substrate composed of multiple metals will introduce lattice distortion due to the difference in atomic volume of different alloy layer elements, thereby improving the activity. At the same time, different alloy layer elements will form a more stable phase, thereby improving the electrochemical stability; it can be seen that the porous metal catalyst formed by the micron porous substrate composed of multiple metals will improve the catalyst activity or stability due to the alloy layering effect.
[0080] In one embodiment, the filler includes: alumina or quartz sand.
[0081] In one embodiment, the second metal and the filler are in powder form.
[0082] In one embodiment, when the micron porous substrate is in a mesh or foam form, the mesh number of the micron porous substrate is 10 to 110 meshes, and when the micron porous substrate is in a felt form, the wire diameter of the micron porous substrate is in a range of 3 μm to 100 μm.
[0083] The mesh, foam or felt-like micron porous substrate is used to increase the specific surface area of the porous metal catalyst. When the mesh number of the micron porous substrate is 10-110 meshes, the specific surface area can be ensured while avoiding the problem of poor electrolyte flow or difficulty in detachment of generated bubbles during water electrolysis.
[0084] In one embodiment, the particle size of the second metal is 120-325 mesh, and the particle size of the filler is 40-325 mesh.
[0085] The second metal or filler is set to the above-mentioned particle size range, mainly based on the consideration of alloy layer uniformity. When the particles of the second metal or filler are too large, it will lead to incomplete contact between the powder and metal A, thus affecting the effect of alloy layer; while too high a powder mesh number will not significantly improve the effect of alloy layer, but significantly increase the price.
[0086] In one embodiment, the mass ratio of the second metal to the filler is: the mixing ratio of the second metal to the filler is 1:1 to 1:3. The filler is used to bond the second metal to the micron porous substrate.
[0087] The micron porous substrate and the second metal are annealed to form an alloy layer on the surface of the micron porous substrate.
[0088] The annealing treatment is used to form an alloy layer on the surface of the microporous substrate by solid thermal diffusion.
[0089] After the alloy layer is formed, the cooled microporous substrate is separated from the mixed powder of the second metal and the filler, and the residual powder of the second metal and the filler on the surface of the microporous substrate is cleaned.
[0090] In one embodiment, there is a difference in saturated vapor pressure between the first metal element and the second metal element, so that the second metal element can be partially or completely sublimated from the alloy layer, thereby achieving a dealloying process and forming a micro-nanoscale porous structure.
[0091] In one embodiment, the alloy layer includes a first metal element and a second metal element, the first metal element includes at least one of Ni, Fe, Cu, Co, Mn, Ti, Cr, Mo, W, Ta, Au, Ag, Nb, Zr, and V; the second metal element includes any one of Zn, Mg, Bi, and Cd.
[0092] The sources of raw materials and equipment involved in the present invention are all raw materials and equipment that can be purchased on the market.
[0093] In one embodiment, the alloy layering equipment includes: a box furnace or a tube furnace.
[0094] In one embodiment, when performing annealing, heating is started after a protective gas is introduced into the alloy layering device for 15 to 30 minutes, and the protective gas is argon or nitrogen. In order to prevent residual oxygen in the furnace chamber from oxidizing the workpiece, heating is started after the protective gas is introduced for 15 to 30 minutes.
[0095] In one embodiment, during the annealing treatment, the alloy layering temperature is 300-500° C., and the holding time is 0.5-5 hours.
[0096] In one embodiment, the thickness of the alloy layer is 10-100 μm.
[0097] The thickness of the alloy layer can be controlled by controlling the temperature and holding time of the alloy layer. In order to ensure the catalytic activity of the porous catalyst finally formed, the alloy layer temperature is controlled to be not less than 300°C, the holding time is not less than 0.5h, and the thickness of the alloy layer is not less than 10μm; at the same time, in order to avoid cracking and falling off of the alloy layer, the alloy layer temperature is controlled to be not higher than 500°C, the holding time is not less than 5h, and the thickness of the alloy layer is not less than 100μm.
[0098] The micron porous substrate with an alloy layer formed on the surface is placed in a vacuum heat treatment device for vacuum heat treatment to form a porous metal catalyst.
[0099] The second metal element in the alloy layer will partially or completely sublime out of the alloy layer due to the difference in saturated vapor pressure between the first metal element and the second metal element, and the remaining elements in the alloy layer will self-assemble to form a micro-nano scale porous structure, thereby obtaining a porous metal catalyst having a specific shape of a micron porous substrate itself and a micro-nano porous layer formed after the surface is dealloyed by vacuum heat treatment.
[0100] In one embodiment, the conditions of the vacuum heat treatment are: air pressure lower than 50 Pa, temperature range is 450° C. to 850° C., and insulation time is 0.5 h to 3.5 h.
[0101] In one embodiment, the size range of the ligaments in the porous metal catalyst is 100 nm to 2.5 μm.
[0102] By changing the temperature, duration and vacuum degree of vacuum heat treatment, the ligament size of the micro-nano porous structure can be controlled. When the insulation time is less than 0.5 hours, it is difficult to form a porous structure and the catalytic activity cannot be guaranteed; when the insulation time is longer than 3.5 hours, the porous structure will be significantly coarsened, which will reduce the specific surface area of the porous metal catalyst and thus the catalytic activity. The preparation of porous catalysts with ligament sizes below 100nm is very difficult and difficult to achieve; when the ligament size is higher than 2.5μm, the specific surface area decreases and the catalytic activity will decrease.
[0103] In one embodiment, the micron porous substrate comprises a first characteristic metal, and after the alloy layer is formed on the surface of the micron porous substrate, the method further comprises:
[0104] The micron porous substrate with an alloy layer formed on the surface is placed in an acid solution for corrosion to obtain a metal catalyst with three-level porous characteristics.
[0105] The micron porous substrate with an alloy layer formed on the surface is placed in an acidic solution for corrosion, so as to further increase the specific surface area of the porous metal catalyst, improve the catalytic activity, and at the same time ensure the mechanical strength of the porous metal catalyst.
[0106] In one embodiment, the first characteristic metal includes two or more micron porous base elements, and at least one element among the two or more micron porous base elements is Mn element.
[0107] In one embodiment, the acidic solution is ammonium sulfate.
[0108] In one embodiment, the concentration of ammonium sulfate is greater than or equal to 0.5 M. This is because if the concentration of ammonium sulfate is lower than 0.5 M, the reaction rate will be too slow. It has been verified by experiments that the reaction rate is more suitable when the concentration of ammonium sulfate is 0.5 M-2 M.
[0109] In summary, the present invention provides a method for preparing a porous metal catalyst, by forming an alloy layer on the surface of a micron porous substrate, and forming pores in the alloy layer by vacuum heat treatment, so that the porous metal catalytic electrode prepared by this method only has a porous structure in the alloy layer on the surface, and the original shape of the micron porous substrate is not destroyed, and no subsequent processing and forming process is required. Compared with gas phase alloy layering, the time required to prepare an alloy layer of the same thickness is shorter and more efficient, while improving the activity of the porous metal catalyst, it also ensures the mechanical strength of the porous metal catalyst structure.
[0110] The technical solution provided by the present invention can also control the thickness of the alloy layer by changing the time and temperature of the surface alloying layer, and can control the ligament size of the porous structure by controlling the temperature, duration and vacuum degree of the vacuum heat treatment.
[0111] In addition, the preparation method described in the present invention does not require the use of various chemical reagents such as acids, alkalis and salts, and the sublimated metal vapor during the vacuum heat treatment process can be recovered through a condensation device and reused repeatedly after treatment, so it has less impact on the environment, lower production costs, and is easier to carry out large-scale production.
[0112] According to one embodiment of the present invention, there is provided a porous metal catalyst, comprising:
[0113] The micron porous substrate has an alloy layer formed by the first metal element and the second metal on its surface, the alloy layer also includes a filler, and the alloy layer has micro-nano pores.
[0114] In one embodiment, in the alloy layer, the molar percentage of the first metal element is 20%-50%; the molar percentage of the second metal element is 50%-80%.
[0115] The porous metal catalyst provided by the present invention forms a micro-nano porous alloy layer on the surface of a micron porous substrate, thereby improving the activity of the porous metal catalyst, and the micron porous substrate ensures the mechanical strength of the porous metal catalyst. Therefore, the technical solution provided by the present invention improves the catalytic activity of the porous metal catalyst while also ensuring the mechanical strength of the porous metal catalyst structure.
[0116] In one embodiment, the alloy layer further includes nanoscale pores.
[0117] The specific surface area of the porous metal catalyst is 75 to 95 m 2 / g.
[0118] The nanoscale pores, the microscale pores in the micrometer porous substrate, and the micro-nanoscale pores in the alloy layer form a three-level porous catalyst structure, which increases the specific surface area of the porous metal catalyst and greatly improves the catalytic activity of the porous metal catalyst.
[0119] In one embodiment, the hole size of the micron-scale porous substrate is 5 μm to 500 μm, the ligament size of the micro-nano porous substrate is 0.1 μm to 10 μm, and the ligament size of the nano-scale porous substrate is 10 nm to 99 nm.
[0120] It can be seen that the technical solution provided by the present invention improves the catalytic activity while ensuring the mechanical strength of the porous metal catalyst.
[0121] According to one embodiment of the present invention, a method for preparing an electrode catalyst assembly is provided, including the method for preparing the porous metal catalyst according to any one of the aforementioned embodiments of the present invention.
[0122] According to one embodiment of the present invention, there is further provided a catalytic electrode assembly, comprising the porous metal catalyst described in the foregoing embodiment of the present invention.
[0123] According to one embodiment of the present invention, there is provided a use of the catalytic electrode assembly as described in the aforementioned embodiment of the present invention in producing hydrogen by hydrolysis.
[0124] The catalytic electrode assembly can be directly applied to the process of producing hydrogen by electrolyzing water, and when the catalytic electrode assembly is used as a cathode, it exhibits catalytic activity for the hydrogen evolution reaction and has excellent hydrogen evolution performance and stability.
[0125] In addition, the catalytic electrode assembly can also be used as an anode in the process of producing hydrogen by electrolysis of water. At this time, the catalytic electrode assembly exhibits catalytic activity for the oxygen evolution reaction and has excellent oxygen evolution performance and stability.
[0126] In one embodiment, when the porous metal catalyst is used in a water electrolysis process, the surface hydrogen evolution overpotential is as low as 80-140 mV.
[0127] The following is combined with specific embodiments and reference Figure 2-Figure 8 , a preparation method of a porous metal catalyst provided by the present invention and its performance are described in detail:
[0128] Example 1
[0129] The method for preparing the porous metal catalyst provided in this embodiment includes:
[0130] 1) Cut a metal Ni mesh as a micron porous substrate with a mesh size of 50 meshes; select metal Zn as an alloying element in a powdered form with a particle size of 325 meshes; select alumina (Al2O3) as a filler in a powdered form with a particle size of 325 meshes.
[0131] 2) First put the Ni mesh into the tubular furnace, then evenly mix the Zn powder and Al2O3 powder in a mass ratio of 1:1 and cover the surface of the Ni mesh to ensure that the surface of the Ni mesh is not exposed.
[0132] 3) Argon was selected as the protective gas. After the argon was continuously introduced for 30 min, the Ni mesh covered with the mixed powder was heated in a tubular furnace at a temperature of 500° C. for 0.5 h.
[0133] Figure 2 It is a cross-sectional scanning electron microscope image of a single wire after the surface alloy layer of the Ni mesh and the Zn powder in Example 1 of the present invention and an EDS element surface distribution map of Ni and Zn.
[0134] Please refer to Figure 2 , Zn and Ni will form a Ni-Zn alloy layer on the surface of the Ni mesh through solid thermal diffusion, with a thickness of about 80μm.
[0135] After the surface alloying is completed, the cooled Ni mesh is separated from the mixed powder and the residual powder on the surface is cleaned.
[0136] The cleaned Ni mesh was placed in a vacuum heat treatment furnace for heating at a pressure of 50 Pa, a temperature of 450°C, and a holding time of 3 h.
[0137] Figure 3 is a scanning electron microscope image of the micro-nano porous metal Ni mesh obtained after vacuum heat treatment in Example 1 of the present invention (the inset is a local enlarged image), Figure 4 is its XRD diffraction pattern.
[0138] Please refer to Figure 3 and Figure 4 ,After vacuum heat treatment, a porous structure is formed on the surface of the Ni mesh, the ligament size is 300-500nm, and the element composition is 92at.% Ni, 8at.% Zn.
[0139] Figure 5 It is a linear scanning diagram of the hydrogen evolution reaction on the surface of the micro-nano porous metal Ni mesh in Example 1 of the present invention.
[0140] Please refer to Figure 5 When the micro-nano porous metal Ni mesh is made into a catalytic electrode for water electrolysis, a linear scanning diagram of hydrogen evolution reaction on the surface of the micro-nano porous metal Ni mesh is obtained, wherein the potential relative to the reversible hydrogen electrode is the abscissa, the unit is: V; the current density is the ordinate, the unit is: mA / cm2 ,Depend on Figure 5 It can be seen that when the potential at 10 mA / cm2 is used as the hydrogen evolution overpotential of the cathode catalytic electrode assembly, the surface hydrogen evolution overpotential of the cathode catalytic electrode assembly is 110 mV.
[0141] Figure 6 : is a linear scan diagram of the oxygen evolution reaction on the surface of the micro-nano porous metal Ni mesh in Example 1 of the present invention. Figure 6 It can be seen that when the potential at 20 mA / cm2 is used as the oxygen evolution overpotential of the anode catalytic electrode assembly, the surface oxygen evolution overpotential of the anode catalytic electrode assembly is 326 mV.
[0142] Example 2
[0143] The method for preparing the porous metal catalyst provided in this embodiment includes:
[0144] 1) Cut a certain size of metal Ni felt as a micron porous substrate, with a wire diameter of 35 μm. Select metal Zn as an alloying element, in the form of powder with a particle size of 325 mesh. Select alumina (Al2O3) as a filler, in the form of powder with a particle size of 200 mesh.
[0145] 2) First put the Ni felt into the tubular furnace, then evenly mix the Zn powder and Al2O3 powder in a mass ratio of 1:2 and cover the surface of the Ni felt to ensure that the surface of the Ni felt is not exposed.
[0146] 3) Nitrogen was selected as the protective gas. After nitrogen was continuously introduced for 20 minutes, the Ni felt covered with the mixed powder was heated in a tube furnace at 400°C for 0.5 hours. Zn and Ni formed a Ni-Zn alloy layer on the surface of the Ni felt by thermal diffusion, with a thickness of about 15 μm. After the surface alloy layer was formed, the cooled Ni felt was separated from the mixed powder and the residual powder on the surface was cleaned.
[0147] 4) Place the cleaned Ni felt in a vacuum heat treatment furnace and heat it at a pressure of 10 -3 Pa, temperature 600℃, holding time 1.5h.
[0148] Figure 6 This is a scanning electron microscope image of the micro-nano porous metal Ni felt obtained after vacuum heat treatment in Example 2 of the present invention (the inset is a local enlarged image).
[0149] Please refer to Figure 6 ,After vacuum heat treatment, a porous structure is formed on the surface of Ni felt, the ligament size is 400-600nm, and the element composition is 95at.% Ni, 5at.% Zn.
[0150] When the micro-nano porous metal Ni felt is used as a catalytic electrode for water electrolysis, the surface hydrogen evolution overpotential is 80 mV.
[0151] Example 3
[0152] The method for preparing the porous metal catalyst provided in this embodiment includes:
[0153] 1) Cut a certain size of Ni-Cu alloy layer mesh as a micron porous substrate, the mesh number is 50 mesh. Select metal Zn as an alloying element, its shape is powder, and the particle size is 325 mesh. Select quartz sand (SiO2) as a filler, its shape is powder, and the particle size is 200 mesh.
[0154] 2) First, place the Ni-Cu alloy layer mesh into a box furnace, and then evenly mix the Zn powder and SiO2 powder in a mass ratio of 1:2 and cover the surface of the Ni-Cu alloy layer mesh to ensure that the surface of the Ni-Cu alloy layer mesh is not exposed.
[0155] 3) Argon is selected as the protective gas. After continuously passing argon for 30 minutes, the Ni-Cu alloy layer mesh covered with the mixed powder is heated in a tube furnace at a temperature of 450°C for 0.5 hours. Zn, Ni and Cu will form a Ni-Cu-Zn alloy layer on the surface of the Ni-Cu alloy layer mesh by thermal diffusion, with a thickness of about 60 μm. After the surface alloying is completed, the cooled Ni-Cu alloy layer mesh is separated from the mixed powder and the residual powder on the surface is cleaned.
[0156] 4) Place the cleaned Ni-Cu alloy layer mesh in a vacuum heat treatment furnace and heat it at a pressure of 10 -2 Pa, temperature 550℃, holding time 1.5h.
[0157] Figure 7 This is a scanning electron microscope image of the micro-nano porous Ni-Cu alloy layer network obtained after vacuum heat treatment in Example 3 of the present invention (the inset is a local enlarged image), Figure 8 is its XRD diffraction pattern.
[0158] Please refer to Figure 7 and Figure 8 ,After vacuum heat treatment, a porous structure is formed on the surface of the Ni-Cu alloy layer mesh, the ligament size is 450-600nm, and the element composition is 66at.%Ni, 27at.%Cu, 7at.%Zn.
[0159] When the micro-nano porous Ni-Cu alloy layer network is used as a catalytic electrode for water electrolysis, the surface hydrogen evolution overpotential is 140mV.
[0160] Example 4
[0161] The method for preparing the porous metal catalyst provided in this embodiment includes:
[0162] 1) Cut a certain size of Ni-Mo-Cr-Fe alloy layer mesh as a micron porous substrate, the mesh number is 40 mesh. Select metal Zn as an alloying element, the shape of which is powder, and the particle size is 325 mesh. Select alumina (Al2O3) as a filler, the shape of which is powder, and the particle size is 325 mesh.
[0163] 2) First, place the Ni-Mo-Cr-Fe alloy layer mesh into a box furnace, and then evenly mix the Zn powder and Al2O3 powder in a mass ratio of 1:1 and cover the surface of the Ni-Mo-Cr-Fe alloy layer mesh to ensure that the surface of the Ni-Mo-Cr-Fe alloy layer mesh is not exposed.
[0164] 3) Select argon as the protective gas. After continuously introducing argon for 30 minutes, heat the Ni-Mo-Cr-Fe alloy layer mesh covered with the mixed powder in a box furnace at a temperature of 400°C for 4 hours. Zn and Ni, Fe, Mo, and Cr will form a Ni-Mo-Cr-Fe-Zn alloy layer on the surface of the Ni-Mo-Cr-Fe alloy layer mesh by thermal diffusion. The thickness is about 70μm. After the surface alloying is completed, separate the cooled Ni-Mo-Cr-Fe alloy layer mesh from the mixed powder and clean the residual powder on the surface.
[0165] 4) Place the cleaned Ni-Mo-Cr-Fe alloy layer mesh in a vacuum heat treatment furnace and heat it at a pressure of 10 -3 Pa, temperature 650℃, holding time 1h.
[0166] Fig. 9 This is a scanning electron microscope image of the micro-nano porous Ni-Mo-Cr-Fe alloy layer network obtained after vacuum heat treatment in Example 4 of the present invention (the inset is a local enlarged view), Fig.10 Its XRD diffraction pattern.
[0167] Please refer to Fig. 9 and Fig.10 After vacuum heat treatment, a porous structure is formed on the surface of the Ni-Mo-Cr-Fe alloy layer network, the ligament size is 100-300nm, and the element composition is 61at.%Ni, 15at.%Cr, 9at.%Mo, 7at.%Fe, 8at.%Zn, such as Fig. 9 When the micro-nano porous Ni-Mo-Cr-Fe alloy layer network is used as a catalytic electrode for water electrolysis, the surface hydrogen evolution overpotential is 101mV and the surface oxygen evolution overpotential is 200mV.
[0168] Example 5
[0169] The method for preparing the porous metal catalyst provided in this embodiment includes:
[0170] 1) Cut a certain size of Ni-Fe-Cr alloy layer mesh as a micron porous substrate, the mesh number is 100 mesh. Select metal Zn as an alloying element, its shape is powder, and the particle size is 325 mesh. Select alumina (Al2O3) as a filler, its shape is powder, and the particle size is 325 mesh.
[0171] 2) First, place the Ni-Fe-Cr alloy layer mesh into a tubular furnace, and then evenly mix the Zn powder and the Al2O3 powder in a mass ratio of 1:3 and cover the surface of the Ni-Fe-Cr alloy layer mesh to ensure that the surface of the Ni-Fe-Cr alloy layer mesh is not exposed.
[0172] 3) Argon is selected as the protective gas. After continuously introducing argon for 30 minutes, the Ni-Fe-Cr alloy layer mesh covered with the mixed powder is heated in a tube furnace at a temperature of 500°C for 0.5 hours. Zn, Ni, Fe, and Cr will form a Ni-Fe-Cr-Zn alloy layer on the surface of the Ni-Fe-Cr alloy layer mesh by thermal diffusion, with a thickness of about 50 μm. After the surface alloying is completed, the cooled Ni-Fe-Cr alloy layer mesh is separated from the mixed powder and the residual powder on the surface is cleaned.
[0173] 4) Place the cleaned Ni-Fe-Cr alloy layer mesh in a vacuum heat treatment furnace and heat it at an air pressure of 10 -2 Pa, temperature 550℃, holding time 2.5h.
[0174] Fig.11 This is a scanning electron microscope image of the micro-nano porous Ni-Fe-Cr alloy layer network obtained after vacuum heat treatment in Example 5 of the present invention (the inset is a local enlarged view).
[0175] Please refer to Fig.11 ,After vacuum heat treatment, a porous structure is formed on the surface of the Ni-Fe-Cr alloy layer mesh, the ligament size is 300-400nm, and the element composition is 68at.% Ni, 18at.% Cr, 9at.% Fe, 5at.% Zn.
[0176] When the micro-nano porous Ni-Fe-Cr alloy layer network is used as a catalytic electrode for water electrolysis, the surface hydrogen evolution overpotential is 132 mV.
[0177] Example 6
[0178] Compared with Examples 1 to 5, this embodiment further corrodes the Ni mesh with a porous structure on the surface into an acidic solution to form a catalyst with a three-level porous structure. Specifically, the preparation method of the porous metal catalyst provided in this embodiment includes:
[0179] 1) Cut a metal Ni-Mn alloy mesh as the first metal with a mesh size of 50 meshes; select metal Zn as the alloying element in the form of powder with a particle size of 325 meshes; select alumina (Al2O3) as the filler in the form of powder with a particle size of 325 meshes.
[0180] 2) First, place the Ni-Mn alloy mesh into a tubular furnace, and then evenly mix the Zn powder and the Al2O3 powder in a mass ratio of 1:1 and cover the surface of the metal mesh to ensure that the surface of the metal mesh is not exposed.
[0181] 3) Argon was selected as the protective gas. After the argon was continuously introduced for 30 minutes, the Ni-Mn alloy mesh covered with the mixed powder was heated in a tubular furnace at a temperature of 500° C. for 0.5 hours.
[0182] Zn, Ni and Mn will form a Ni-Mn-Zn alloy layer on the surface of the Ni-Mn alloy mesh through solid thermal diffusion, and the thickness is about 80 μm.
[0183] After the surface alloying is completed, the cooled Ni alloy mesh is separated from the mixed powder and the residual powder on the surface is cleaned.
[0184] The cleaned Ni mesh was placed in a vacuum heat treatment furnace for heating at a pressure of 50 Pa, a temperature of 450°C, and a holding time of 3 h.
[0185] The Ni mesh with porous structure on the surface is placed in an acidic solution: ammonium sulfate with a concentration of 0.5M to 2M for corrosion, and a metal catalyst with three-level porous characteristics is obtained, and its ligament structure is composed of crystals, such as Fig.12 shown.
[0186] After vacuum heat treatment and free corrosion, a three-level porous structure is formed on the surface of the Ni mesh, the ligament size is 20-30nm, and the element composition is 88at.%Ni, 8.2at.%Zn, and 3.5at.%Mn.
[0187] Comparative Example 1
[0188] Comparative Example 1 is a nickel mesh with Raney nickel sprayed on the surface. Fig.13 The scanning electron microscope image of the nickel mesh with Raney nickel sprayed on the surface of Comparative Example 1 of the present invention (the inset is a local enlarged view); the linear scanning diagram of the hydrogen evolution reaction on its surface is as follows Fig.14 As shown, its surface hydrogen evolution overpotential is 182mV.
[0189] In Examples 1 to 5, micron porous substrates with different structures and compositions were respectively provided, and cathode catalytic electrode assemblies were obtained under different alloy temperatures, times, vacuum heat treatment temperatures, times, etc., and applied to the process of electrolysis of water to obtain the surface hydrogen evolution overpotentials of the cathode catalytic electrode assemblies in Examples 1 to 5. Figure 3 , Figure 5-Figure 8 It can be seen that Examples 1 to 5 all have relatively low surface hydrogen evolution overpotentials. The surface hydrogen evolution overpotential of Comparative Example 1 is greater than that of Examples 1 to 5 provided by the present invention. Compared with Comparative Example 1, the cathode catalytic electrode assembly provided by Examples 1 to 5 above not only ensures the mechanical strength of the cathode catalytic electrode assembly, but also greatly improves the catalytic activity of the cathode catalytic electrode assembly.
[0190] Compared with Examples 1 to 5, the Ni mesh in Example 6 was placed in an acidic solution: ammonium sulfate with a concentration of 0.5M to 2M for corrosion, and a metal catalyst with a three-level porous feature was obtained. As a cathode catalytic electrode assembly, the surface hydrogen evolution pass point obtained by testing is lower, and the catalytic activity is far better than the cathode catalytic electrode assembly in Examples 1-5.
[0191] It can be seen from Examples 1 and 4 that the porous metal catalyst provided in the embodiments of the present invention can be used as both a cathode and an anode in a hydrolysis hydrogen production process. When used as a cathode, it exhibits catalytic activity for the hydrogen evolution reaction, and when used as an anode, it exhibits catalytic activity for the oxygen evolution reaction.
[0192] In summary, the technical solution provided by the present invention improves the activity of the porous metal catalyst while ensuring the mechanical strength of the porous metal catalyst structure. Compared with gas phase alloying, it takes less time and is more efficient to prepare an alloy layer of the same thickness. In addition, the preparation method of the present invention has less impact on the environment, lower production costs, and is easier to carry out large-scale production.
[0193] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a porous metal catalyst, characterized in that: include: providing a microporous substrate, a second metal, and a filler; mixing the second metal and a filler to form a mixture; Putting the micron porous substrate into an alloying device, wherein the micron porous substrate has a shape of a mesh, a foam or a felt; Covering the mixture on the surface of the microporous substrate; After covering the surface of the microporous substrate with the mixture, annealing the microporous substrate and the second metal to form an alloy layer on the surface of the microporous substrate; The micron porous substrate with the alloy layer formed on the surface is placed in a vacuum heat treatment device for vacuum heat treatment to form a porous metal catalyst.
2. The method for preparing a porous metal catalyst according to claim 1, characterized in that: During annealing, the alloy layering temperature is 300°C to 500°C, and the holding time is 0.5h to 5h.
3. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The thickness of the alloy layer is 10 μm to 100 μm.
4. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The conditions of the vacuum heat treatment are: air pressure lower than 50 Pa, temperature range of 450° C. to 850° C., and heat preservation time of 0.5 h to 3.5 h.
5. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The ligament size range in the porous metal catalyst is 100nm~2.5μm.
6. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The filler includes: alumina or quartz sand. 7 . The method for preparing a porous metal catalyst according to claim 1 , wherein the second metal and the filler are in powder form.
8. The method for preparing a porous metal catalyst according to claim 7, characterized in that: When the micron porous substrate is in a mesh or foam form, the mesh number of the micron porous substrate is 10 to 110 meshes. When the micron porous substrate is in a felt form, the wire diameter of the micron porous substrate is in a range of 3 μm to 100 μm.
9. The method for preparing a porous metal catalyst according to claim 7, characterized in that: The particle size of the second metal is 120-325 meshes, and the particle size of the filler is 40-325 meshes.
10. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The mass ratio of the second metal to the filler is: the mixing ratio of the second metal to the filler is 1:1 to 1:
3.
11. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The alloy layering equipment includes: a box furnace or a tube furnace.
12. The method for preparing a porous metal catalyst according to claim 1, characterized in that: When performing annealing treatment, a protective gas is introduced into the alloy layering equipment for 15 to 30 minutes before starting heating. The protective gas is argon or nitrogen.
13. The method for preparing a porous metal catalyst according to claim 1, characterized in that: The micron porous substrate comprises a first characteristic metal. After a porous metal catalyst is formed on the surface of the micron porous substrate, the method further comprises: The micron porous substrate with porous metal catalyst formed on the surface is placed in an acid solution for corrosion to obtain a metal catalyst with three-level porous characteristics.
14. The method for preparing a porous metal catalyst according to claim 13, characterized in that: The first characteristic metal includes two or more micron porous base elements, and at least one element among the two or more micron porous base elements is Mn or Al.
15. The method for preparing a porous metal catalyst according to claim 13, characterized in that: The acidic solution is ammonium sulfate.
16. The method for preparing a porous metal catalyst according to claim 15, characterized in that: The concentration of the ammonium sulfate is greater than or equal to 0.5M.
17. The method for preparing a porous metal catalyst according to claim 1, wherein the alloy layer comprises a first metal element and a second metal element, wherein the first metal element comprises at least one of Ni, Fe, Cu, Co, Mn, Ti, Cr, Mo, Al, W, Ta, Au, Ag, Nb, Zr, and V; and the second metal element comprises: Any one of Zn, Mg, Bi, and Cd.
18. A method for preparing an electrode catalyst assembly, comprising the method for preparing the porous metal catalyst according to any one of claims 1 to 17.
19. A porous metal catalyst, characterized in that: include: The micron porous substrate has an alloy layer formed by a first metal element and a second metal on its surface, the alloy layer also includes a filler, and the alloy layer has micro-nano pores.
20. The porous metal catalyst according to claim 19, characterized in that In the alloy layer, the molar percentage of the first metal element is 20%-50%; the molar percentage of the second metal element is 50%-80%.
21. The porous metal catalyst according to claim 19, characterized in that The alloy layer also includes nano-scale pores.
22. The porous metal catalyst according to claim 21, characterized in that The specific surface area of the porous metal catalyst is 75 to 95 m 2 / g.
23. The porous metal catalyst according to claim 22, characterized in that The hole size of the micron-scale porous substrate is 5 μm to 500 μm, the ligament size of the micro-nano porous substrate is 0.1 μm to 10 μm, and the ligament size of the nano-scale porous substrate is 10 nm to 99 nm.
24. A catalytic electrode assembly, characterized in that: Comprising the porous metal catalyst according to claim 15 or 17.
25. Use of the catalytic electrode assembly according to claim 18 in producing hydrogen by hydrolysis.
26. Use of the catalytic electrode assembly according to claim 25 in producing hydrogen by hydrolysis, characterized in that: The catalytic electrode assembly exhibits catalytic activity for oxygen evolution reaction.
27. Use of the catalytic electrode assembly according to claim 25 in producing hydrogen by hydrolysis, characterized in that: The catalytic electrode assembly exhibits catalytic activity for hydrogen evolution reaction.
Citation Information
Patent Citations
Porous binary Ni-Mn oxide lithium battery negative electrode material and preparation method thereof
CN107958992A
Porous catalytic electrode for hydrogen production by hydrolysis and preparation method of porous catalytic electrode
CN117626331A
A fabrication method of NANO porous metal
KR101561966B1
Cited By
Nano-porous composite electro-catalytic material as well as preparation method and application thereof
CN119913551A
Porous metal catalyst and preparation method therefor
WO2026026628A1