Photocathode with CO2 adsorption capacity and photoelectrocatalysis CO2 reduction as well as preparation method and application of photocathode
By constructing the Cu2O@Bi2O3/Si photocathode, using the tight p-n heterojunction and interface atomic localization effect, the problem of insufficient photoelectro-catalytic performance and CO2 adsorption properties of Bi2O3 is solved, and more efficient carbon dioxide reduction performance and lower The reduction starting potential significantly improves the photoelectrocatalytic performance.
Patent Information
- Application Number
- CN202410967218.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Bi2O3 has defects such as wide bandgap, low carrier mobility and high overpotential during photoelectro-catalytic carbon dioxide reduction, which leads to its limited application in PEC-CO2RR, and the diverse crystal surfaces of Cu2O lead to diverse reduction products and susceptibility to light. Corrosion, low CO2 adsorption performance.
The Cu2O@Bi2O3/Si photocathode was constructed by hydrothermal method and static coating method to form a tight p-n heterojunction. The rapid electron transfer mechanism of the contact interface was used to accelerate the transfer of Cu2O photoelectrons to Bi2O3, and the atomic localization was achieved through the p-n junction interface. The effect builds electron-rich sites to improve the photoelectric properties and CO2 adsorption properties of the catalyst.
Significantly improves CO2 adsorption and photoelectrochemical reduction performance, the current density of Cu2O@Bi2O3/Si photocathode is enhanced by about 5 times at -0.3V vs RHE bias voltage, with lower reduction starting potential and better CO2 localization It has a enrichment ability and can stabilize carbon dioxide reduction to formic acid.
Smart Images

Figure CN118957654A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of photoelectrocatalysis, and relates to a photocathode and a preparation method and application thereof, and specifically relates to a Bi- 2 O 3 @Cu 2 O / Si photocathode and its preparation method and application. Background Art
[0002] Photoelectrocatalysis is an effective combination of the advantages of photocatalysis and electrocatalysis. Semiconductors are used as photocathodes or photoanodes. Under light, the semiconductor electrode generates electron holes that are used to react with CO. 2 Reduction reaction, while adding additional negative potential to the system (which can be provided by clean energy such as wind energy and solar energy), on the one hand, can effectively separate semiconductor photogenerated electron-hole pairs to promote the reaction, and on the other hand, can effectively control the reaction products by changing the potential. Therefore, photoelectrocatalysis is an effective way to utilize solar energy, which can reduce carbon dioxide in the air to liquid fuels with higher economic value, such as formic acid, acetic acid, ethanol, etc.
[0003] At present, bismuth-based materials have been confirmed to be CO due to their flexible coordination structure and low HER activity. 2 The ideal material for the reduction of formic acid. In particular, Bi-MOF-based Bi-derived 2 O 3 Not only does it retain highly dispersed active sites, but the derived carbon substrate also alleviates the Bi 2 O 3 However, Bi 2 O 3 The inherent defects such as wide band gap, low carrier mobility and high overpotential have not been effectively overcome, which hinders its application in PEC-CO 2 RR applications. Therefore, it is urgent to construct a reasonable heterojunction to improve Bi 2 O 3 The optoelectronic properties of Cu with narrow band gap and high carrier density 2 O is an excellent photoelectron donor, but when it is used as an active site, its diverse crystal faces lead to a large number of reduction products. 2 O is easily reduced by untransferred photoelectrons, resulting in severe photocorrosion. Inspired by the above, if we construct a reasonable close pn heterojunction and utilize the fast electron transfer mechanism of the contact interface to accelerate the Cu 2 O photoelectron transfer to Bi 2 O 3 Conduct CO 2At the same time, the atomic localization effect of the pn junction interface is used to construct electron-rich sites, which may take into account both the photoelectric properties of the catalyst and the CO 2 Improved adsorption. Summary of the invention
[0004] The current photocathode in photoelectrocatalytic CO 2 The low performance of the reduction and the CO 2 The present invention provides a method for improving CO 2 Adsorption performance and good CO 2 Photoelectrochemical reduction of bismuth-based metal-organic framework-derived Cu 2 O@Bi 2 O 3 / Si photocathode, which has a stronger carbon dioxide enrichment ability, can accelerate the adsorption and activation of carbon dioxide molecules, and stabilize the key intermediates in the carbon dioxide reduction process. In addition, the photocathode has excellent photoelectrochemical properties and has good application prospects in the field of photoelectrocatalytic carbon dioxide reduction.
[0005] The purpose of the present invention is achieved by at least one of the following technical solutions.
[0006] A CO 2 Adsorption capacity and photoelectrocatalytic CO 2 The reduced photocathode is prepared by a hydrothermal method and carbonized in an inert atmosphere.
[0007] The present invention has a CO 2 Adsorption capacity and photoelectrocatalytic CO 2 The preparation method of the reduced photocathode, the specific preparation steps are as follows:
[0008] (1) preparing a bismuth-based metal-organic framework material Bi-MOF as a precursor: adding an active metal source and an organic metal ligand 1,3,5-trimethylbenzene trimesic acid to an organic solution, stirring continuously until completely dissolved, transferring the obtained precursor solution to a polytetrafluoroethylene liner, placing the precursor in a stainless steel reactor under an electric oven for reaction, and after the reaction is completed, taking out the reactor and cooling it at room temperature, and repeatedly washing the product with deionized water, drying, rolling and screening it to obtain a bismuth-based metal-organic framework material;
[0009] (2) dispersing the precursor material obtained in step (1) in deionized water, slowly adding a metal source solution, stirring, centrifuging to obtain a precipitate, repeatedly washing with deionized water, and drying to obtain a metal-modified bismuth-based metal-organic framework material; the metal source contains at least one element of Bi and Cu;
[0010] (3) carbonizing the metal-modified bismuth-based metal organic framework material obtained in step (2) under an inert gas atmosphere to obtain Cu 2 O@Bi 2 O 3 catalyst;
[0011] (4)Configure Cu 2 O@Bi 2 O 3 Ethanol (containing 1% Nafion) dispersion solution, Cu was coated by static coating method. 2 O@Bi 2 O 3 Loaded on Si wafer, it is used for photoelectrocatalytic CO 2 Reduced Cu 2 O@Bi 2 O 3 / Si photocathode.
[0012] Further preferably, in step (1), the active metal salt is one of bismuth nitrate or bismuth acetate.
[0013] Further preferably, in step (1), the amount of the active metal source added is 0.5 to 1.0 mmol; the amount of the organic metal ligand 1,3,5-trimethylbenzenecarboxylic acid added is 0.1 to 0.3 mmol; the temperature of the electric oven is 100 to 150° C., and the reaction time is 8 to 16 h.
[0014] Further preferably, in step (2), the concentration of the precursor powder is 1-5 g / L, the concentration of the metal source solution is 5-20 mmol / L, the amount of the metal source solution added is 50-100 mL; and the stirring time is 6-12 h.
[0015] Further preferably, in step (2), the copper source is copper nitrate, the copper source concentration is 5 to 20 mmol, and the addition amount is 50 to 100 mL.
[0016] Further preferably, in step (3), the carbonization temperature is 200-500°C, the time is 1-4h; the inert gas is N 2 , flow rate 180ml / min.
[0017] Further preferably, in step (4), Cu 2 O@Bi 2 O 3 The concentration of the ethanol dispersion solution is 0.2 to 1.0 mg / mL.
[0018] Further preferably, in step (4), the Cu 2 O@Bi 2 O 3The ethanol dispersion solution contains 1% Nafion.
[0019] More preferably, in step (4), the static coating is performed 20 to 50 times.
[0020] Further preferably, in step (4) Cu 2 O@Bi 2 O 3 The concentration of the powder solution is 0.2 to 1.0 mg / mL, and the number of static pulling times is 20 to 50 times.
[0021] The present invention also provides that within the low potential range, the potential interval of the photocathode for reducing carbon dioxide to obtain formic acid is -0.1 to -0.55 V vs RHE.
[0022] Compared with the prior art, the advantages of the present invention are:
[0023] (1) Compared with the original Bi 2 O 3 Compared with the Cu / Si photocathode, the Cu 2 O@Bi 2 O 3 The current density of the Si / Si pnp junction photocathode at a bias of -0.3 V vs RHE is enhanced by about 5 times, and it has better photoelectrocatalytic reduction of carbon dioxide performance and lower reduction onset potential.
[0024] (2) Cu constructed by the present invention 2 O@Bi 2 O 3 / Si pnp junction photocathode has better CO 2 The local enrichment capacity is the original Bi 2 O 3 / about 5 times that of Si photocathode.
[0025] (3) The present invention adopts a hydrothermal method and a static pulling method to prepare the photocathode, which does not require a complicated coating process. The prepared photocathode has excellent photoelectrochemical performance and the ability to reduce carbon dioxide to formic acid. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Preparation of the photoelectrocatalytic CO 2 Reduced Cu 2 O@Bi 2 O 3 / Si photocathode SEM image.
[0027] Figure 2 Preparation of the photoelectrocatalytic CO 2 Reduced Cu 2 O@Bi2 O 3 TEM image of.
[0028] Figure 3 Example 2 was used to prepare the photoelectrocatalytic CO 2 Reduced Cu 2 O@Bi 2 O 3 UV-visible absorption spectrum of Si / Si photocathode.
[0029] Figure 4 Example 2 was used to prepare the photoelectrocatalytic CO 2 Reduced Cu 2 O@Bi 2 O 3 / Si photocathode transient photocurrent curve.
[0030] Figure 5 Example 2 was used to prepare the photoelectrocatalytic CO 2 Reduced Cu 2 O@Bi 2 O 3 / Si photocathode LSV curve.
[0031] Figure 6 Bi prepared in Example 3 2 O 3 @Cu 2 O / Si photocathode for photocatalytic reduction of CO 2 Faradaic efficiency for the production of formic acid.
[0032] Figure 7 Preparation of Cu for photoelectrocatalytic carbon dioxide reduction in Example 3 2 O@Bi 2 O 3 / Si photocathode for photoelectrocatalytic reduction of CO 2 Prepare the NMR spectrum of formic acid.
[0033] Figure 8 Preparation of Cu for photoelectrocatalytic carbon dioxide reduction in Example 3 2 O@Bi 2 O 3 / Si photocathode active component Cu 2 O@Bi 2 O 3 CO 2 -TPD image. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with the accompanying drawings and specific examples. It should be understood that these examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0035] Example 1
[0036] Cu 2 O@Bi 2 O 3 Preparation of Si photocathode
[0037] (1) First, a bismuth-based metal organic framework material is prepared as a precursor by a hydrothermal method in the prior art, and the specific steps are as follows:
[0038] 1) Weigh 1.2 g of trimesic acid and 0.89 g of bismuth nitrate pentahydrate, stir and dissolve in 60 mL of an organic solvent (methanol: N,N-dimethylformamide = 3:1), stir vigorously, then transfer to a polytetrafluoroethylene liner, heat at 120° C. for 12 hours, centrifuge, wash, and vacuum dry at 80° C. overnight to obtain a bismuth-based metal organic framework material as a precursor material.
[0039] 2) Weigh 0.2 g of bismuth-based metal organic framework precursor powder and ultrasonically disperse it in 100 ml of deionized water, and add 5-20 mmol / L copper nitrate solution drop by drop. Further stir vigorously for 6 hours, collect the precipitate by centrifugation, wash it with deionized water, and vacuum dry it at 80°C for 12 hours.
[0040] 3) placing the copper-loaded bismuth-based metal organic framework precursor powder in a tube furnace under N 2 The metal organic framework derivative was obtained by calcining at 300 °C for 3 h in an atmosphere and recorded as Cu 2 O@Bi 2 O 3 .
[0041] Figure 1 The Cu prepared in this example 2 O@Bi 2 O 3 TEM image of heterojunction material, Cu 2 O is uniformly anchored in the Bi-based metal-organic framework-derived Bi 2 O 3 Surface, Cu 2 The particle size of O particles is about 50nm.
[0042] (2) Cu 2 O@Bi 2 O 3 Cu is loaded on the Si surface 2 O@Bi 2O 3 / Si photocathode
[0043] 1) Weigh 0.01g Cu 2 O@Bi 2 O 3 The powder material was dispersed in 5 ml of anhydrous ethanol (50 ul 5% Nafion). Ultrasonication was performed for 30 min until it was completely dispersed. 2 O@Bi 2 O 3 The powder concentration is 0.2 mg / ml.
[0044] 2) A layer of Cu is applied on the surface of the Si electrode by a static pulling instrument. 2 O@Bi 2 O 3 The pulling times are 20 to 50 times. Finally, Cu 2 O@Bi 2 O 3 / Si photocathode.
[0045] Figure 2 The Cu prepared in this example 2 O@Bi 2 O 3 SEM image of the Cu / Si photocathode. 2 O@Bi 2 O 3 The particles are uniformly loaded in the porous Si electrode, and the larger Cu 2 O@Bi 2 O 3 The particles are loaded on the surface of Si electrode.
[0046] Example 2
[0047] Cu 2 O@Bi 2 O 3 Photoelectrochemical performance of / Si photocathode
[0048] The Cu prepared in Example 1 2 O@Bi 2 O 3 The / Si photocathode was tested in a UV-visible spectrophotometer. The photoelectrochemical performance was tested in an electrochemical workstation under a three-electrode system. 2 O@Bi 2 O 3 / Si photocathode as the working electrode, Pt sheet as the counter electrode, Ag / AgCl as the reference electrode, and electrolysis is also CO 2 Saturated 0.5M KHCO 3The solution was illuminated by a 300W xenon lamp with a light intensity of 200mW cm -2 .
[0049] Figure 3 The Cu prepared in this example 2 O@Bi 2 O 3 UV-visible absorption spectrum of Si photocathode, showing that there is no Cu 2 O loaded Bi 2 O 3 The light absorption intensity of Si photocathode is lower than that of Cu 2 O@Bi 2 O 3 / Si photocathode. 2 O@Bi 2 O 3 / Si photocathode shows full spectrum absorption and has stronger light absorption intensity.
[0050] Figure 4 The Cu prepared in this example 2 O@Bi 2 O 3 / Si photocathode transient photocurrent spectrum. As can be seen from the figure, at 200mW cm -2 Visible light irradiation, -0.3V vs RHE, no Cu 2 O loaded Bi 2 O 3 The photocurrent of the Si photocathode is only 2.4 mA cm -2 , and Cu 2 O@Bi 2 O 3 / Si photocurrent is 6.7mAcm -2 , indicating that the Cu prepared in this example 2 O@Bi 2 O 3 / Si photocathode has excellent photoelectric conversion efficiency.
[0051] Example 3
[0052] Cu 2 O@Bi 2 O 3 Photoelectrocatalytic CO / Si photocathode 2 Restore performance
[0053] The Cu prepared in Example 1 2 O@Bi 2 O 3 / Si photocathode for photoelectrocatalytic CO in a closed H-Cell electrolyzer 2Reduction performance test. High-purity CO is continuously introduced during the test. 2 gas to saturate the electrolyte. 2 O@Bi 2 O 3 The / Si photocathode was used as the working electrode, the Pt sheet was used as the counter electrode, and the Ag / AgCl was used as the reference electrode. The Faradaic efficiency of the reduction product was analyzed by measuring the concentration of the reduction product.
[0054] Figure 5 The Cu prepared in this example 2 O@Bi 2 O 3 Linear sweep voltammetry curve of / Si photocathode. As can be seen from the figure, the original Si electrode has no CO 2 reduction activity, thus showing poor voltage-current response. 2 O@Bi 2 O 3 / Si photocathode has better CO 2 Reduction performance, compared with no Cu 2 O-anchored Bi 2 O 3 / Si photocathode, overpotential decreased by 219mV (10mA cm -2 ).
[0055] Figure 6 The Cu prepared in this example 2 O@Bi 2 O 3 The product Faraday efficiency of the / Si photocathode at different test potentials. As can be seen from the figure, formic acid is the main reduction product at different test potentials. At -0.3V vs RHE, the formic acid Faraday efficiency is as high as 94.0%. CO and H 2 As a byproduct, the Faraday efficiency is low.
[0056] Figure 7 The Cu prepared in this example 2 O@Bi 2 O 3 / Si photocathode liquid phase product nuclear magnetic resonance hydrogen spectrum (NMR) analysis at -0.3VvsRHE potential. As can be seen from the figure, only formic acid can be detected in the electrolyte after the reaction, and no other liquid phase products are detected, indicating that Cu 2 O@Bi 2 O 3 / Si photocathode due to the photoelectrocatalytic CO 2 Reduction to formic acid performance.
[0057] Figure 8 The Cu prepared in this example 2 O@Bi2 O 3 The active component Cu in the Si photocathode 2 O@Bi 2 O 3 Temperature programmed desorption of carbon dioxide (CO 2 -TPD) curve. Cu 2 O@Bi 2 O 3 Higher CO in high temperature areas 2 The desorption peak indicates that it is higher than Bi 2 O 3 With stronger CO 2 Chemical adsorption capacity.
[0058] It should be understood that the above detailed description of the technical solution of the present invention with the help of optimized embodiments is illustrative rather than restrictive, and it cannot be determined that the specific implementation methods of the present invention are limited to this. For ordinary technicians in the technical field to which the present invention belongs, without departing from the concept of the present invention, modifications to the technical solutions recorded in the embodiments, or equivalent replacement of some of the technical features therein, should be deemed to fall within the scope of patent protection determined by the claims submitted for the present invention.
[0059] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction, characterized in that: Prepared by hydrothermal method and carbonized in inert atmosphere; The specific steps include: (1) preparing a bismuth-based metal-organic framework material (Bi-MOF) as a precursor: adding an active metal source and an organic metal ligand 1,3,5-trimethic acid to an organic solution, stirring continuously until completely dissolved, transferring the obtained precursor solution to a polytetrafluoroethylene liner, placing the precursor solution in a stainless steel reactor under an electric oven for reaction, and after the reaction is completed, taking out the reactor and cooling it at room temperature, and repeatedly washing the reaction product with deionized water, drying, rolling and screening to obtain a bismuth-based metal-organic framework material; (2) dispersing the precursor material obtained in step (1) in deionized water, slowly adding a metal source solution, stirring, centrifuging to obtain a precipitate, repeatedly washing with deionized water, and drying to obtain a metal-modified bismuth-based metal-organic framework material; the metal source contains at least one element of Bi and Cu; (3) carbonizing the metal-modified bismuth-based metal organic framework material obtained in step (2) under an inert gas atmosphere to obtain a Cu2O@Bi2O3 catalyst; (4) A Cu2O@Bi2O3 ethanol dispersion solution was prepared, and Cu2O@Bi2O3 was loaded on a Si wafer by a static coating method to obtain a Cu2O@Bi2O3 / Si photocathode for photoelectrocatalytic CO2 reduction.
2. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (1), the active metal salt is one of bismuth nitrate or bismuth acetate.
3. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (1), the amount of the active metal source added is 0.5 to 1.0 mmol; the amount of the organic metal ligand 1,3,5-trimethylbenzenecarboxylic acid added is 0.1 to 0.3 mmol; the temperature of the electric oven is 100 to 150° C., and the reaction time is 8 to 16 hours.
4. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (2), the concentration of the precursor powder is 1-5 g / L, the concentration of the metal source solution is 5-20 mmol / L, and the amount of the metal source solution added is 50-100 mL; the stirring time is 6-12 h.
5. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (3), the carbonization temperature is 200 to 500° C. and the time is 1 to 4 hours.
6. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (4), the concentration of the Cu2O@Bi2O3 ethanol dispersion solution is 0.2-1.0 mg / mL.
7. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (4), the Cu2O@Bi2O3 ethanol dispersion solution contains 1% Nafion.
8. The method for preparing a photocathode having CO2 adsorption capacity and photoelectrocatalytic CO2 reduction according to claim 1, characterized in that: In step (4), the static coating is performed 20 to 50 times.
9. The preparation method according to any one of claims 1 to 8 prepares a Cu2O@Bi2O3 / Si photocathode with CO2 adsorption capacity and photoelectrocatalytic CO2 reduction.
10. The Cu2O@Bi2O3 / Si photocathode of claim 9 is applied to CO2 adsorption and photoelectrocatalytic CO2 reduction, characterized in that: The photoelectrocatalytic reduction of carbon dioxide to formic acid was tested in the potential range of -0.1 to -0.55 V vs RHE.
Citation Information
Patent Citations
Preparation method and application of alpha-Bi2O3 / CuBi2O4 heterojunction photocatalytic material synthesized in situ
CN111420668A
Preparation method and application of bismuth-based metal organic framework material
CN117166000A
Hierarchical pore titanium silicalite loaded copper-bismuth bimetallic catalyst, preparation method thereof and method for preparing methanol through photoelectrocatalysis CO2 reduction by using hierarchical pore titanium silicalite loaded copper-bismuth bimetallic catalyst
CN117512614A
Cited By